Activated waste rubber powder and preparation method thereof as well as modified asphalt and preparation method thereof
A technology of waste rubber powder and modified asphalt, which is applied to building components, building insulation materials, buildings, etc., can solve the problems of time-consuming industrial production, complicated process, difficult operation, etc., and achieves convenient operation, simple process, good phase capacitive effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0034] The preparation method of the activated waste rubber powder of the present invention comprises: kneading a mixture containing waste rubber powder, a softener and / or a rubber activator at a temperature of 50-100° C. for 10-20 minutes to obtain activated waste rubber powder. The mixing can be carried out in a rubber mixing machine, which can be various equipment known to those skilled in the art that can be used for mixing, for example, it can be open, closed, or it can be a screw rubber mixing machine.
[0035] The waste rubber powder modified asphalt of the present invention is made from a mixture containing matrix asphalt and activated waste rubber powder, and the activated waste rubber powder is the activated waste rubber powder provided by the present invention. Moreover, the content of the base asphalt is 75-92% by weight, and the content of the activated waste rubber powder is 8-25% by weight.
[0036] In the waste rubber powder modified asphalt of the present inv...
Embodiment 1-9
[0047] 1. Preparation of activated waste rubber powder
[0048] The activated waste rubber powder of embodiment 1-12 is prepared by the components listed in table 1 and the consumption thereof, and each component is added in the rubber mixing machine (Shanghai rubber machinery factory, SK-1608), and in table 1 Mixing is carried out under the listed mixing temperature and mixing time to obtain activated waste rubber powder.
[0049] Table 1
[0050]
waste rubber powder
(parts by mass)
softener
(parts by mass)
rubber activator
(parts by mass)
Mixing temperature
(℃)
Mixing time
(minute)
Example 1
80 mesh
100 copies
naphthenic oil
3.5 servings
-
50
20
Example 2
80 mesh
100 copies
-
De-link
1 copy
100
10
Example 3
80 mesh
100 copies
naphthenic oil
3.6 servings ...
PUM
Property | Measurement | Unit |
---|---|---|
particle size (mesh) | aaaaa | aaaaa |
softening point | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com