Method for synthesis of alicyclic epoxy resin with catalysis of solid supported heteropoly acid catalyst
A technology of immobilized heteropolyacid and epoxy resin, which is applied in the field of immobilized heteropolyacid catalyst to catalyze the synthesis of alicyclic epoxy resin, can solve the problems of low yield, poor synthesis process safety, catalyst residue, etc. The effect of high efficiency and purity, low cost and good safety
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0024] Example 1 The process for the synthesis of epoxy resin ERL-4221 catalyzed by the immobilized heteropolyacid catalyst is as follows:
[0025] Synthesis of immobilized phosphotungstic acid catalyst: add 2Kg chloromethyl polystyrene resin to 6L N,N-dimethylformamide (DMF) to swell for 2 hours, then add 8L tertiary amine R 1 R 2 R 3 N(R 1 , R 2 , R 3 is alkyl, cycloalkyl or benzyl) at 90-100°C for 24 hours, then cooled the reaction mixture, filtered it with suction, and washed the filter cake with water and ethanol in turn, then extracted with ethanol for 8-10 hours, and then vacuumed Dry to constant weight, make immobilized quaternary ammonium resin, this immobilized quaternary ammonium resin can be represented as respectively or in Represents chloromethyl polystyrene resin carrier;
[0026] Weigh 825g of phosphotungstic acid and dissolve it in 10L of water, stir the reaction, and take 1.5L of 30% H 2 o 2 Add to the reaction solution in 5 times, control the re...
Embodiment 2
[0037] Example 2 The process of the solid-supported heteropolyacid catalyst catalyzing the synthesis of dicyclopentadiene dioxide is as follows:
[0038]
[0039] Synthesis of immobilized phosphomolybdic acid catalyst: add 1.5Kg of bromomethyl polystyrene resin to 5L of dimethyl sulfoxide (DMSO) to swell for 3 hours, then add 6L of pyridine or its homologous compounds and stir at a temperature of 80-90°C After 20 hours, the reaction mixture was cooled, filtered with suction, and the filter cake was washed with water and ethanol in turn, then extracted with ethanol for 9 to 10 hours, and then dried in vacuum to constant weight to obtain a solid-loaded quaternary ammonium salt resin;
[0040] Take by weighing 30g phosphomolybdic acid and be dissolved in 500mL water, stir reaction, and take 350mL mass percent concentration and be 50% H 2 o 2 Add to the reaction solution in 5 times, control the reaction temperature at about 20°C, react for 6 hours, and adjust the pH value of t...
Embodiment 3
[0042] Embodiment 3 The technological process of this immobilized heteropolyacid catalyst catalytic synthesis of 4-vinyl epoxycyclohexane is as follows:
[0043]
[0044] Synthesis of immobilized phosphovanadic acid catalyst: add 200g fluoromethyl polystyrene resin to 0.5L N,N-dimethylformamide (DMF) to swell for 4h, then add 0.3L piperidine or its homologous compound at 100°C Stir at high temperature for 18 hours, then cool the reaction mixture, filter with suction, wash the filter cake with water and ethanol in turn, then extract with ethanol for 10 hours, and then dry it in vacuum to constant weight to obtain a solid-loaded quaternary ammonium salt resin;
[0045] Take by weighing 10g phosphovanadic acid and be dissolved in 150mL water, stir reaction, and take 120mL mass percent concentration and be 40% H 2 o 2 Add to the reaction solution in 5 times, control the reaction temperature at about 50°C, react for 3 hours, and adjust the pH value of the reaction solution to <...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology