Method for manufacturing polyisophthaloyl metaphenylene diamide pulp-shaped fibre
A poly-m-phenylene isophthalamide and pulp technology is applied in the field of preparing poly-m-phenylene isophthalamide pulp-like fibers, and can solve the problems of unfavorable aramid paper, complicated process and production process. long and other issues
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] Embodiment 1. is that the DMAc solution of the polym-phenylene isophthalamide that concentration is 8wt%, resin inherent viscosity is 1.5 is heated to 50 ℃, and is composed of DMAc40wt%, glycerol 20wt%, water The 40wt% precipitant is mixed and solidified into pulp-like fibers rapidly in the forming equipment. The rotational speed of the forming equipment is 2000 rpm, and it is kept for 10 minutes. The sediment is washed, filtered and dried to obtain the pulp-like polyresorcin Formamide m-phenylenediamide fiber with a specific surface area of 28.6m 2 / g, the average length is 2.2mm, and the aspect ratio is 70-80.
[0021] In this example, the mass ratio of the precipitating agent to polym-phenylene isophthalamide is 30:1.
Embodiment 2
[0022] Embodiment 2. is that the NMP solution of polym-phenylene isophthalamide that concentration is 8wt%, resin inherent viscosity is 1.55 is heated to 50 ℃, and is composed of NMP38wt%, ethylene glycol 40wt%, water The precipitant of 22wt% is mixed in forming equipment and solidifies rapidly into pulp-like fiber, and the rotational speed of forming equipment is 2400 rev / mins, keep 12 minutes, sediment is washed, filtered, dried, obtains pulp-like polyresorcin Formamide m-phenylenediamide fiber with a specific surface area of 31.9m 2 / g, the average length is 3.0mm, and the aspect ratio is 65-79.
[0023] In this embodiment, the mass ratio of the precipitating agent to polym-phenylene isophthalamide is 45:1.
Embodiment 3
[0024] Embodiment 3. is that the DMAc solution of polym-phenylene isophthalamide that concentration is 7.8wt%, resin inherent viscosity is 1.52 is heated to 50 ℃, and is composed of DMAc25wt%, ethylene glycol 24wt%, The precipitating agent of 51wt% of water is mixed in the forming equipment and solidified rapidly into pulp-like fibers. The rotating speed of the forming equipment is 1800 rpm, and it is kept for 9 minutes, and the precipitate is washed, filtered and dried to obtain pulp-like polymethane Diformyl m-phenylenediamide fiber with a specific surface area of 26.4m 2 / g, the average length is 2.0mm, and the aspect ratio is 48-67.
[0025] In this example, the mass ratio of the precipitating agent to polym-phenylene isophthalamide is 20:1.
PUM
Property | Measurement | Unit |
---|---|---|
shear viscosity | aaaaa | aaaaa |
viscosity | aaaaa | aaaaa |
shear viscosity | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com