An algae inhibitor and fishing net technology, which is applied in the fields of botanical equipment and methods, herbicides, algaecides, biocides, etc. Promotion and application and other issues to achieve the effect of reducing breeding costs, saving manpower and time, and shortening the breeding cycle
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] Get 10 grams of tetrachloroisophthalonitrile and add 15 grams of cosolvent propylene glycol and add 5 grams of water and 0.2 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 12 hours;
[0031] Take 5 grams of pyrithione, add 7 grams of cosolvent propylene glycol, add 2 grams of water and 0.1 gram of surfactant nonylphenol polyoxyethylene ether, and mix them uniformly with a ball mill for 12 hours;
[0032] Get 5 grams of thiocyanomethane and add 7 grams of cosolvent propylene glycol and add 2 grams of water and 0.1 gram of surfactant nonylphenol polyoxyethylene ether and mix evenly with a ball mill for 12 hours;
[0033] Add 50 grams of acrylic resin to 30 grams of water and mix well;
[0034] Take 0.3 grams of calcium polyacrylate and add 2 grams of water and mix well;
[0035] The above solutions are combined and stirred evenly, and the pH value is adjusted to 7.0-10.0 to obtain an anti-algae agent product for fishing nets o...
Embodiment 2
[0037] Get 5 grams of tetrachloroisophthalonitrile and add 10 grams of cosolvent propylene glycol and add 5 grams of water and 0.1 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 11 hours;
[0038] Take 10 grams of pyrithione, add 15 grams of cosolvent propylene glycol, add 8 grams of water and 0.2 grams of surfactant nonylphenol polyoxyethylene ether, and mix them uniformly with a ball mill for 11 hours;
[0039] Get 8 grams of thiocyanomethane and add 10 grams of cosolvent propylene glycol and add 5 grams of water and 0.1 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 11 hours;
[0040] Add 60 grams of acrylic resin to 40 grams of water and mix well;
[0041] Take 0.2 grams of calcium polyacrylate and add 2 grams of water to mix evenly;
[0042] The above solutions are combined and stirred evenly, and the pH value is adjusted to 7.0-10.0 to obtain an anti-algae agent product for fishing...
Embodiment 3
[0044] Get 15 grams of tetrachloroisophthalonitrile and add 20 grams of cosolvent propylene glycol and add 10 grams of water and 0.3 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 13 hours;
[0045] Take 2 grams of pyrithione, add 4 grams of cosolvent propylene glycol, add 2 grams of water and 0.05 grams of surfactant nonylphenol polyoxyethylene ether, and mix them uniformly with a ball mill for 13 hours;
[0046] Get 10 grams of thiocyanomethane and add 15 grams of cosolvent propylene glycol and add 10 grams of water and 0.2 gram of surfactant nonylphenol polyoxyethylene ether and mix uniformly with a ball mill for 13 hours;
[0047] Add 70 grams of acrylic resin to 50 grams of water and mix well;
[0048] Take 0.4 gram of polyacrylic acid calcium and add 2 grams of water and mix well;
[0049] The above solutions are combined and stirred evenly, and the pH value is adjusted to 7.0-10.0 to obtain an anti-algae agent product for fi...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com