High-accuracy high-moulding brass strip and processing technology thereof
A processing technology, brass strip technology, applied in the direction of metal rolling, can solve the problems of poor stability of brass strip, affecting processing efficiency, unfavorable use, etc., to ensure uniformity of texture and structural performance, improve internal and surface Performance, easy to generate processing effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0060] A high-precision and high-shape brass strip and its processing technology, the brass strip processing technology includes the following steps:
[0061] P1. Smelting: add raw materials according to the specified ratio, perform multiple smelting in the smelting furnace, remove scum, and obtain molten raw materials;
[0062] P2. Pouring: pouring the molten raw material into the mold to form a pouring billet;
[0063] P3. Preliminary rolling: place the cast billet in the rolling mill for preliminary rolling to form a brass plate;
[0064]P4. Intermediate annealing: use an annealing furnace to anneal the brass plate, the annealing temperature is 450 degrees Celsius to 550 degrees Celsius, the heating time is 2 hours to 3 hours, and the heat preservation is 8 hours to 12 hours to 60 degrees Celsius to 70 degrees Celsius, and the annealed plate is obtained ;
[0065] P5. Pre-finish rolling: place the annealed plate in the rolling mill for pre-finish rolling to the remaining ...
Embodiment 2
[0086] A high-precision and high-shape brass strip and its processing technology, the brass strip processing technology includes the following steps:
[0087] P1. Smelting: add raw materials according to the specified ratio, perform multiple smelting in the smelting furnace, remove scum, and obtain molten raw materials;
[0088] P2. Pouring: pouring the molten raw material into the mold to form a pouring billet;
[0089] P3. Preliminary rolling: place the cast billet in the rolling mill for preliminary rolling to form a brass plate;
[0090] P4. Intermediate annealing: use an annealing furnace to anneal the brass plate, the annealing temperature is 450 degrees Celsius to 550 degrees Celsius, the heating time is 2 hours to 3 hours, and the heat preservation is 8 hours to 12 hours to 60 degrees Celsius to 70 degrees Celsius, and the annealed plate is obtained ;
[0091] P5. Pre-finish rolling: place the annealed plate in the rolling mill for pre-finish rolling to the remaining...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com