A method for preparing aramid nanofibers
A nanofiber, para-aramid fiber technology, applied in fiber raw material processing, textile and papermaking, etc., can solve the problems of low reaction concentration, long reaction period, shortened reaction period, etc. Effects of large proton exchange rates
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0033] (1) Add 1g of para-aramid fibers with an average length of 4mm and 1.5g of KOH into 500ml of DMSO solution, and place them in a 1000ml beaker;
[0034] (2) Place the beaker containing the para-aramid fiber, KOH and DMSO mixed system obtained in step (1) in a water bath, and use an ultrasonic cell breaker to perform ultrasonic treatment to obtain ultrasonically treated para-aramid fiber Suspension A; the processing conditions are: ultrasonic power 300W, ultrasonic treatment time 150min, ultrasonic working time: 4s, ultrasonic interval: 2s; further, add ice cubes continuously to ensure that the temperature of the water bath is maintained below 40°C.
[0035](3) Add water in the para-aramid fiber suspension A obtained in step (2), the volume of the added water is 2.5:1ml / g with the ratio of the absolute dry mass of the para-aramid fiber to obtain Para-aramid fiber suspension B.
[0036] (4) After sealing the para-aramid fiber suspension B obtained in step (3), place the a...
Embodiment 2
[0039] (1) Add 1g of para-aramid fibers with an average length of 5mm and 1.5g of KOH into 500ml of DMSO solution, and place them in a 1000ml beaker;
[0040] (2) Place the beaker containing the para-aramid fiber, KOH and DMSO mixed system obtained in step (1) in a water bath, and use an ultrasonic cell breaker to perform ultrasonic treatment to obtain ultrasonically treated para-aramid fiber Suspension A; the processing conditions are: ultrasonic power 400W, ultrasonic treatment time 120min, ultrasonic working time: 4s, ultrasonic interval: 2s; further, add ice continuously to ensure that the temperature of the water bath is maintained below 40°C.
[0041] (3) Add water in the para-aramid fiber suspension A obtained in step (2), the volume of the added water is 5:1ml / g with the ratio of the absolute dry mass of the para-aramid fiber to obtain Para-aramid fiber suspension B.
[0042] (4) Place the para-aramid fiber suspension B obtained in step (3) after being sealed and stir...
Embodiment 3
[0045] (1) Add 1g of para-aramid fibers with an average length of 6mm and 1.5g of KOH into 500ml of DMSO solution, and place them in a 1000ml beaker;
[0046] (2) Place the beaker containing the para-aramid fiber, KOH and DMSO mixed system obtained in step (1) in a water bath, and use an ultrasonic cell breaker to perform ultrasonic treatment to obtain ultrasonically treated para-aramid fiber Suspension A; the processing conditions are: ultrasonic power 500W, ultrasonic treatment time 90min, ultrasonic working time: 4s, ultrasonic interval: 2s; further, add ice cubes continuously to ensure that the temperature of the water bath is maintained below 40°C.
[0047] (3) Add water in the para-aramid fiber suspension A obtained in step (2), the volume of the added water is 8:1ml / g with the ratio of the absolute dry weight of the para-aramid fiber to obtain Para-aramid fiber suspension B.
[0048] (4) After sealing the para-aramid fiber suspension B obtained in step (3), place it in...
PUM
Property | Measurement | Unit |
---|---|---|
length | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com