Magnetic isolation sheet for wireless charging and preparation method thereof
A technology of wireless charging and magnetic isolation sheet, which is applied in the direction of inorganic material magnetism, can solve the problems of high loss and low Bs of magnetic isolation sheet, and achieve the effect of high Bs and low loss
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0041] The embodiment of the present application provides a preparation method of a magnetic isolation sheet for wireless charging, the preparation method comprising:
[0042] S101: The raw materials for preparing the magnetic isolation sheet are Fe according to the mass ratio 2 o 3 69.5%, Mn 3 o 4 23% and ZnO7.5% are uniformly mixed and then tableted to obtain raw material tablets.
[0043] S102: Pre-fire the raw material sheet at a temperature of 950°C until the tap density of the pre-fired raw material sheet is 1.3 g / cm 3 .
[0044] S103: Pulverize the calcined raw material pieces to form a pulverized material.
[0045] S104: Mix crushed materials, auxiliary materials, polyvinyl alcohol glue and deionized water to form a mixture. The rotational speed of the mixture was sand-milled at 2000r / min, the sand-milling time was 180min, and the sand-milled particle size was 0.8μm. The auxiliary materials include calcium carbonate, vanadium pentoxide, niobium pentoxide, elemen...
Embodiment 2
[0053] The embodiment of the present application provides a preparation method of a magnetic isolation sheet for wireless charging, the preparation method comprising:
[0054] S201: The raw materials for preparing the magnetic isolation sheet are Fe according to the mass ratio 2 o 3 69.5%, Mn 3 o 4 23% and ZnO7.5% are uniformly mixed in proportion and then tableted to obtain raw material tablets.
[0055] S202: Pre-fire the raw material sheet at a temperature of 948°C until the tap density of the pre-fired raw material sheet is 1.5 g / cm 3 .
[0056] S203: Pulverize the calcined raw material pieces to form a pulverized material.
[0057] S204: Mix crushed materials, auxiliary materials, polyvinyl alcohol glue and deionized water to form a mixture. The rotation speed of the mixture was 2000r / min, the sanding time was 120min, and the sanding time was 1.4μm. The auxiliary materials include calcium carbonate, vanadium pentoxide, niobium pentoxide, elemental iron and dicobalt...
Embodiment 3
[0065] The embodiment of the present application provides a preparation method of a magnetic isolation sheet for wireless charging, the preparation method comprising:
[0066] S301: The raw materials for preparing the magnetic isolation sheet are Fe according to the mass ratio 2 o 3 65%, MnO26% and ZnO9% are uniformly mixed in proportion and then tableted to obtain raw material tablets.
[0067] S302: Pre-fire the raw material sheet at a temperature of 945°C until the tap density of the pre-fired raw material sheet is 1.3g / cm 3 .
[0068] S303: Pulverize the calcined raw material pieces to form a pulverized material.
[0069] S304: Mix crushed materials, auxiliary materials, polyvinyl alcohol glue and deionized water to form a mixture. The rotational speed of the mixture was sand-milled at 2000r / min, the sand-milling time was 90min, and the sand-milled particle size was 1.2μm. The auxiliary materials include calcium carbonate, vanadium pentoxide, niobium pentoxide, elemen...
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
particle size | aaaaa | aaaaa |
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com