3003H14 aluminum alloy sheet and production method thereof

A technology of aluminum alloy plate and production method, which is applied in the field of aluminum alloy manufacturing, can solve the problems that the surface quality cannot meet the requirements of high-end products, the surface quality cannot meet the requirements of high-end products, and the temperature control of the annealing furnace is poor, so as to save cold rolling and annealing Process, save production time, improve the effect of surface and shape quality

Inactive Publication Date: 2018-05-22
CHINALCO RUIMIN
View PDF6 Cites 3 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] At present, the process flow of 3003H14 aluminum alloy plate is: melting and casting—sawing—ingot heating—hot rolling—cold rolling—intermediate annealing—finished product cold rolling—cross cutting—packaging, the process is lengthy, the processing cost is high, and the surface quality cannot be satisfied Demand for high-end products
In order to ensure intermediate annealing and finished product performance, the thickness after hot rolling should reserve enough processing space for cold rolling. The hot rolling thickness is large and the efficiency is low; when using intermediate annealing, the temperature control of the annealing furnace is poor, which is easy to cause defects such as coarse grains; The rolling oil remaining on the surface of the strip after cold rolling is prone to defects such as brown annealing oil spots during intermediate annealing, and the surface quality cannot meet the requirements of high-end products

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • 3003H14 aluminum alloy sheet and production method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0032] A chemical composition of a 3003H14 aluminum alloy plate: by mass percentage, Si: 0.063%, Fe 0.455%, Cu: 0.079%, Mn: 1.097%, Mg: 0.008%, Cr: 0.045%, Zn: 0.006%, Ti : 0.017%, other impurities ≤ 0.01%, all impurities ≤ 0.15%, the balance is Al;

[0033] A production method of 3003H14 aluminum alloy plate, using aluminum ingot as raw material, through melting and casting, sawing, face milling, ingot heating, hot rolling (hot rough rolling, hot finish rolling), cold rolling, cleaning and straightening and cross shearing ,Specific steps are as follows:

[0034] 1) Melting and casting: Aluminum ingots are used as raw materials to obtain ingots after melting and casting. The melting temperature is 730°C, the refining temperature is 725°C, and the casting temperature is 685°C;

[0035] 2) Heating the ingot obtained in step 1) after sawing and face milling, the heating temperature of the ingot is 510°C, and the holding time is 4h;

[0036] 3) Hot rolling: use four-high reversi...

Embodiment 2

[0044] A chemical composition of a 3003H14 aluminum alloy plate: by mass percentage, Si 0.080%, Fe: 0.441%, Cu: 0.074%, Mn: 1.148%, Mg: 0.038%, Cr: 0.003%, Zn: 0.009%, Ti : 0.016%, other impurities ≤ 0.01%, all impurities ≤ 0.15%, the balance is Al;

[0045] A production method of 3003H14 aluminum alloy plate, using aluminum ingot as raw material, through melting and casting, sawing, face milling, ingot heating, hot rolling (hot rough rolling, hot finish rolling), cold rolling, cleaning and straightening and cross shearing ,Specific steps are as follows:

[0046] 1) Melting and casting: Aluminum ingots are used as raw materials to obtain ingots after melting and casting. The melting temperature is 735°C, the refining temperature is 725°C, and the casting temperature is 689°C;

[0047] 2) Heating the ingot obtained in step 1) after sawing and face milling, the heating temperature of the ingot is 505°C, and the holding time is 5h;

[0048] 3) Hot rolling: use four-high reversi...

Embodiment 3

[0054] A chemical composition of a 3003H14 aluminum alloy plate, by mass percentage, Si: 0.121%, Fe: 0.493%, Cu: 0.089%, Mn: 1.090%, Mg: 0.009%, Cr: 0.031%, Zn: 0.007%, Ti: 0.015%, other impurities ≤ 0.01%, all impurities ≤ 0.15%, the balance is Al;

[0055] A production method of 3003H14 aluminum alloy plate, using aluminum ingot as raw material, through melting and casting, sawing, face milling, ingot heating, hot rolling (hot rough rolling, hot finish rolling), cold rolling, cleaning and straightening and cross shearing ,Specific steps are as follows:

[0056] 1) Melting and casting: Aluminum ingots are used as raw materials to obtain ingots after melting and casting. The melting temperature is 740°C, the refining temperature is 735°C, and the casting temperature is 695°C;

[0057] 2) Heating the ingot obtained in step 1) after sawing and face milling, the heating temperature of the ingot is 510°C, and the holding time is 6h;

[0058] 3) Hot rolling: use four-high reversi...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
thicknessaaaaaaaaaa
tensile strengthaaaaaaaaaa
yield strengthaaaaaaaaaa
Login to View More

Abstract

The invention provides a 3003H14 aluminum alloy sheet and a production method thereof. The 3003H14 aluminum alloy sheet comprises the following components in percentage by mass: less than or equal to0.20% of Si, 0.40-0.50% of Fe, less than or equal to 0.15% of Cu, 1.05-1.20% of Mn, less than or equal to 0.05% of Mg, less than or equal to 0.05% of Cr, less than or equal to 0.10% of Zn, 0.01-0.05%of Ti, less than or equal to 0.05% of other single impurity, less than or equal to 0.15% of all impurities in all and the balance being Al. The production method comprises the following steps: carrying out fusion casting, saw cutting, face-milling, ingot casting heating, hot rolling, cold rolling, cleaning, pulling straightening and transverse shear in sequence. The production method has the beneficial effects that the production method can ensure the performances of the product and shorten the production process; the mechanical properties are controlled by hot rolling plus one-pass cold rolling; and the 3003H14 aluminum alloy sheet product with the thickness of 2.0-4.0mm is produced, and the cost is saved.

Description

technical field [0001] The invention belongs to the technical field of aluminum alloy manufacturing, and in particular relates to a 3003H14 aluminum alloy plate and a production method thereof. Background technique [0002] 3003 aluminum alloy is a kind of rust-proof aluminum widely used in Al~Mn series alloys. Its plate and strip series products have moderate strength, good corrosion resistance, weldability, and easy processing and forming. 3003 aluminum alloy sheets and strips in different heat treatment states are widely used in conductors, cooking utensils, instrument panels, shells and architectural decorations, building materials interior and exterior materials, vehicle interior materials, etc. Among them, the H14 state plate is the largest in terms of consumption and application range. species, the market prospect is broad. [0003] At present, the process flow of 3003H14 aluminum alloy plate is: melting and casting—sawing—ingot heating—hot rolling—cold rolling—inter...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C22C21/00C22C1/02C22F1/04
CPCC22C21/00C22C1/026C22F1/04
Inventor 吴建新乔建博徐始祥冉继龙郑智滨
Owner CHINALCO RUIMIN
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products