A production process and technology for ceramic tiles, applied in the field of ceramic tiles, can solve the problems of limited scope of use, difficult construction of tiles, adverse effects on vision, etc., and achieve low water absorption, rich decoration, brick shape and thermal stability. Good results
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0052] The production process of antique porcelain tiles, including steps:
[0053] A1, take raw materials, carry out slurry ball milling, spray milling, powder bin stale;
[0054] B1, mold compression molding, the prepared slurry is sent into the press mold to be pressed under the condition of 22000MPa, then dried and bisque fired;
[0055]The firing temperature of bisque firing is 1100°, and the firing time is 40 minutes;
[0056] C1, glazing, glaze the surface of the brick adobe;
[0057] The technical parameters of the bottom glaze are as follows: the sieve is 250 mesh sieve, the sieve residue is 0.3g / ml, the specific gravity is 1.78±0.01g / ml, the flow rate is 30±2 seconds, and the glaze amount is 150±1g / piece;
[0058] The technical parameters of the surface glaze are as follows: the sieving is 250 mesh sieve, the sieve residue is 0.3g / ml, the specific gravity is 1.90±0.01g / ml, the flow rate is 35±2 seconds, and the glaze amount is 150±1g / piece.
[0059] D1. Inkjet, pr...
Embodiment 2
[0063] The production process of antique porcelain tiles, including steps:
[0064] The production process of antique porcelain tiles, including steps:
[0065] A2. Take raw materials, carry out slurry ball milling, spray milling, and stale powder bins;
[0066] B2, mold compression molding, the prepared slurry is sent into the press mold to be pressed under the condition of 22000MPa, then dried and bisque fired;
[0067] The firing temperature of bisque firing is 1120°, and the firing time is 40 minutes;
[0068] C2, glazing, adding glaze to the surface of the brick;
[0069] The technical parameters of the bottom glaze are as follows: the sieve is 250 mesh sieve, the sieve residue is 0.3g / ml, the specific gravity is 1.78±0.01g / ml, the flow rate is 30±2 seconds, and the glaze amount is 150±1g / piece;
[0070] The technical parameters of the surface glaze are as follows: the sieving is 250 mesh sieve, the sieve residue is 0.3g / ml, the specific gravity is 1.90±0.01g / ml, the f...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com