A kind of functional wood treatment method

A wood treatment and functional technology, applied in wood treatment, wood treatment details, wood low-temperature treatment, etc., can solve the problems of limited wood properties and limited ability of wood mechanical properties, and achieve good mechanical strength, improved mechanical strength, and improved the effect of strength

Active Publication Date: 2019-01-15
浙江润格木业科技有限公司
View PDF6 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] In the prior art, the performance of the wood itself is limited, and it is often modified by infiltrating the interior of the wood through silica sol to improve the mechanical properties of the wood. However, during this process, it is difficult for the silica to completely penetrate into the interior of the wood. limited ability to improve the mechanical properties of wood

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A kind of functional wood treatment method
  • A kind of functional wood treatment method
  • A kind of functional wood treatment method

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0043] A functional wood processing method, including the following steps:

[0044] Step 1: Soak the wood in hot water at 80°C for 12 hours;

[0045] Step 2: Cool down naturally to room temperature, put it in a refrigerator, and refrigerate at -4°C for 12 hours;

[0046] Step 3: Place the frozen wood at room temperature to thaw naturally;

[0047] Step 4: Configure the treatment solution, dissolve the treatment agent in the aqueous solution, the mass ratio of the treatment agent to the solvent water is 1:4, and the treatment agent includes the following parts by weight:

[0048] Nano silica sol: 100 parts

[0049] Glycerides: 10 parts

[0050] Isobutamidine hydrochloride: 3 parts

[0051] N, N-trimethylsilyl diethylamine: 3 parts

[0052] 3-cyanopropyldimethylmethoxysilane: 2 parts

[0053] Bis (p-nitrobenzene) carbonate: 2 parts

[0054] 2,2-Dimethyl-1,3-propanediol mono(hydroxypivalate): 2 parts;

[0055] Step 5: Put the thawed wood into a closed soaking tank, the soaking tank is filled with...

Embodiment 2

[0067] Step 1: Soak the wood in hot water at 80°C for 12 hours;

[0068] Step 2: Cool down naturally to room temperature, put it in a refrigerator, and refrigerate at -4°C for 12 hours;

[0069] Step 3: Place the frozen wood at room temperature to thaw naturally;

[0070] Step 4: Configure the treatment solution, dissolve the treatment agent in the aqueous solution, the mass ratio of the treatment agent to the solvent water is 1:4, and the treatment agent includes the following parts by weight:

[0071] Nano silica sol: 100 parts

[0072] Glycerides: 10 parts

[0073] Isobutamidine hydrochloride: 3 parts

[0074] N, N-trimethylsilyl diethylamine: 3 parts

[0075] 3-cyanopropyldimethylmethoxysilane: 2 parts

[0076] Bis (p-nitrobenzene) carbonate: 2 parts

[0077] 2,2-Dimethyl-1,3-propanediol mono(hydroxypivalate): 2 parts;

[0078] Step 5: Put the thawed wood into a closed soaking tank, the soaking tank is filled with the treatment solution, and the temperature is raised to 60-80°C, and the s...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention discloses a functional wood treatment method. Wood is soaked in hot water of 80 DEG C, is naturally cooled to the room temperature and is put in a refrigerating chamber, refrigerating is carried out for 12 h under the condition with the temperature being -4 DEG C, the frozen wood is put under the room temperature to be naturally unfrozen, a treatment solution is prepared, the unfrozen wood is put into a closed soaking tank, the soaking tank is full of the treatment solution, the temperature is increased, and soaking is carried out for 10 h to 20 h; and standing cooling is carried out to the room temperature, the treatment solution is discharged, the treatment solution on the surface of the wood is cleared away, and the wood is dried. The wood is soaked through the hot water to dredge clearances between the wood, then cooling and refrigerating are carried out, a sizing function can be achieved besides the clearances between the wood are dredged, and a treatment agent can enter the wood more smoothly later. Strength can be reduced through the wood subjected to heat and cold testament, through permeation, heating and aggregation of the treatment agent solution, the treatment agent solution and molecules between the wood are further combined, and the mechanical strength of the wood is improved and even exceeds original strength.

Description

Technical field [0001] The invention relates to the field of wood processing, and more specifically to a functional wood processing method. Background technique [0002] Wood is the lignified tissue formed by plants capable of secondary growth, such as trees and shrubs. After the primary growth of these plants is over, the vascular cambium in the rhizomes begins to move, developing bast outwards and wood inward. Wood is a general term for plant tissues that develop inward from the vascular cambium, including xylem and thin-walled rays. Wood plays a very supportive role in human life. According to the different properties of wood, people use them in different ways. [0003] In the prior art, the performance of wood itself is limited, and silica sol is often used to infiltrate the interior of the wood for modification to improve the mechanical properties of the wood. However, in this process, it is difficult for silica to completely penetrate into the interior of the wood. Thus, ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Patents(China)
IPC IPC(8): B27K5/00B27K3/52B27K3/08
CPCB27K3/08B27K3/52B27K5/0005B27K5/001
Inventor 陈伟星
Owner 浙江润格木业科技有限公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products