Method for preventing thermal yellowness of raw white shirt lining cloth
A technology for shirts and natural whites is applied in the field of thermal yellowing resistance of natural white shirt interlinings. obvious effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0013] An anti-yellowing method of the white shirt interlining, adding two dyes, Ciba Ellinier Blue A-R and Ciba Pura Red 10B, to the finishing solution of the ordinary white shirt interlining, and completing the process by padding and shaping processes Anti-thermal yellowing process; the specific steps are as follows:
[0014] (1) Dissolve 0.0003g of Ciba Ilinier Blue A-R and 0.0003g of Ciba Pura Red 10B in 0.5L of hot water at 70°C and filter to obtain a mixed filtrate, which is then added to 0.8L of in the finishing solution;
[0015] (2) Padding: The padding method of two dipping and two rolling is used for padding. The time of each padding is 5 seconds, and the pressure of the padding car is 0.10MPa;
[0016] (3) Shaping: the shaping process is carried out through the shaping machine, the speed of the shaping machine is 30m / min, and the shaping temperature is 180°C.
[0017] The whiteness of the white shirt interlining in this embodiment is 78% when tested by a whitenes...
Embodiment 2
[0019] An anti-yellowing method of the white shirt interlining, adding two dyes, Ciba Ellinier Blue A-R and Ciba Pura Red 10B, to the finishing solution of the ordinary white shirt interlining, and completing the process by padding and shaping processes Anti-thermal yellowing process; the specific steps are as follows:
[0020] (1) Put 0.001g of Ciba Ilinier Blue A-R and 0.001g of Ciba Pura Red 10B in 1L of hot water at 80°C to fully dissolve and filter to obtain a mixed filtrate, which is added to 0.5L of finishing in the liquid;
[0021] (2) Padding: The padding method of two dipping and two rolling is used for padding. The time of each padding is 10 seconds, and the pressure of the padding car is 0.20MPa;
[0022] (3) Shaping: the shaping process is carried out through the shaping machine, the speed of the shaping machine is 50m / min, and the shaping temperature is 190°C.
[0023] The whiteness of the white shirt interlining in this embodiment is 85% when tested by a white...
Embodiment 3
[0025] An anti-yellowing method of the white shirt interlining, adding two dyes, Ciba Ellinier Blue A-R and Ciba Pura Red 10B, to the finishing solution of the ordinary white shirt interlining, and completing the process by padding and shaping processes Anti-thermal yellowing process; the specific steps are as follows:
[0026] (1) Put 0.0006g of Ciba Ilinier Blue A-R and 0.0006g of Ciba Pura Red 10B in 0.75L of hot water at 75°C to fully dissolve and filter to obtain a mixed filtrate, which is added to 0.7L of in the finishing solution;
[0027] (2) Padding: The padding method of two dipping and two rolling is used for padding. The time of each padding is 7 seconds, and the pressure of the padding car is 0.18MPa;
[0028] (3) Shaping: the shaping process is carried out through the shaping machine, the speed of the shaping machine is 38m / min, and the shaping temperature is 185°C.
[0029] The whiteness of the white shirt interlining in this embodiment is 86% when tested by a...
PUM
Property | Measurement | Unit |
---|---|---|
whiteness | aaaaa | aaaaa |
whiteness | aaaaa | aaaaa |
whiteness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com