Colorful coating for paper used for fruit raising pouch and preparation method thereof
A technology of raw materials and papermaking wastewater, applied in the direction of coating, etc., can solve the problems of single color and difficult to distinguish fruit bagging, and achieve the effect of changing colors, good growth and strong adhesion
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0043] In the embodiment of the present invention, a kind of colorful fruit-raising bagging paper coating, takes by weighing following raw material:
[0044] Pigment 15kg
[0045] Water-based film-forming substance 35kg
[0046] Defoamer 5kg
[0047] Dispersant 4kg
[0048] Preservative 1kg
[0049] Anti-water agent 2kg
[0050] Adhesive 5kg
[0051] 28kg of water.
[0052] Mix the pigment, defoamer, dispersant, and water at 40°C for 1 hour, then raise the temperature to 55°C, add preservatives, water-resistant agents, and adhesives in sequence, continue stirring for 0.5 hours, then cool down to 25°C, add Aqueous film-forming substance, stirred for 0.3h.
Embodiment 2
[0054] In the embodiment of the present invention, a kind of colorful fruit-raising bagging paper coating, takes by weighing following raw material:
[0055] Pigment 22kg
[0056] Water-based film-forming substance 45kg
[0057] Defoamer 10kg
[0058] Dispersant 12kg
[0059] Preservative 5kg
[0060] Anti-water agent 8kg
[0061] Adhesive 16kg
[0062] 39kg of water.
[0063] Mix the pigment, defoamer, dispersant, and water at 45°C for 2 hours, then raise the temperature to 58°C, add preservatives, water-resistant agents, and adhesives in sequence, continue stirring for 0.7 hours, then cool down to 30°C, add Aqueous film-forming substance, stirred for 0.6h.
Embodiment 3
[0065] In the embodiment of the present invention, a kind of colorful fruit-growing bagging paper coating takes the following raw materials:
[0066] Pigment 18kg
[0067] Water-based film-forming material 39kg
[0068] Defoamer 7kg
[0069] Dispersant 7kg
[0070] Preservative 2kg
[0071] Anti-water agent 4kg
[0072] Adhesive 10kg
[0073] 33kg of water.
[0074] Mix and stir the pigment, defoamer, dispersant, and water at 41°C for 1.2h, then raise the temperature to 56°C, add preservatives, water-resistant agents, and adhesives in sequence, continue stirring for 0.55h, and then cool down to 26°C. Add water-based film-forming substance and stir for 0.4h.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com