Concrete water reducing agent prepared from waste leather slag and preparation method of concrete water reducing agent
A technology of concrete water reducing agent and waste dander, which is applied in the field of concrete admixtures, can solve the problems of difficult disposal of waste dander, waste of resources, environmental pollution, etc. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0041] The embodiment of the present invention provides a method for preparing a concrete water-reducing agent by using waste swarf. The method is implemented by the following steps:
[0042] Step 1: Degradation of waste dander:
[0043] Take 1000 parts of clean waste dander by mass, add 200 parts of water, heat to 35℃, add 0.5 part of penetrant JFC, stir for 1 hour, then adjust the pH to 9.5 with 40% by mass sodium hydroxide, add 1 A portion of 2709-alkaline protease was incubated and stirred for 6 hours to obtain a solution for degrading waste dander, which was lowered to room temperature for later use;
[0044] Step 2: Preparation of water reducing agent:
[0045] Add 30 parts of 36% by mass formaldehyde to the degraded dandruff solution prepared in step 1, heat up to 40°C, add 2 parts of 40% by mass sodium hydroxide solution, and add them in portions within 30 minutes 27~30 parts of urea, add 12 parts of sodium sulfite, heat up to 60℃, keep the temperature for 5 hours, cool to 30...
Embodiment 2
[0047] The embodiment of the present invention provides a method for preparing a concrete water-reducing agent by using waste swarf. The method is implemented by the following steps:
[0048] Step 1: Degradation of waste dander:
[0049] Take 120 parts of clean waste dander according to mass parts, add 240 parts of water, heat to 40℃, add 1 part of penetrant JFC, stir for 1.5 hours, then adjust the pH to 10.5 with 40% by mass sodium hydroxide, add 1.2 parts 2709-Alkaline protease, heat and stir for 8 hours to obtain a solution for degrading waste dander, and lower it to room temperature for use;
[0050] Step 2: Preparation of water reducing agent:
[0051] Add 40 parts of 36% by mass formaldehyde to the degraded dandruff solution prepared in step 1, heat up to 50°C, add 5 parts of 40% by mass sodium hydroxide solution, and add them in batches within 60 minutes After adding 30 parts of urea, add 16 parts of sodium sulfite, heat up to 80℃, keep for 7 hours, and cool to 25~30℃. Add 6 p...
Embodiment 3
[0053] The embodiment of the present invention provides a method for preparing a concrete water-reducing agent by using waste swarf, which is realized by the following steps:
[0054] Step 1: Degradation of waste dander:
[0055] Take 110 parts of clean waste dander according to mass parts, add 220 parts of water, heat to 37.5℃, add 0.75 parts of penetrant JFC, stir for 1.25 hours, then adjust the pH to 10 with 40% mass fraction of sodium hydroxide, add 1.1 parts 2709-Alkaline protease, heat and stir for 7 hours to obtain a solution for degrading waste dander, which is lowered to room temperature for use;
[0056] Step 2: Preparation of water reducing agent:
[0057] Add 35 parts of 36% by mass formaldehyde to the degraded dandruff solution prepared in step 1, heat up to 45°C, add 3.5 parts of 40% by mass sodium hydroxide solution, and add them in 45 minutes. 58 parts of melamine, after adding, the reaction is kept for 45 minutes, then 8 parts of sodium bisulfite are added, the tempe...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com