Process for dyeing silk interwoven jacquard fabric
A technology for jacquard fabric and silk is applied in the field of silk interwoven jacquard fabric dyeing, which can solve the problems of increasing water cost and waste water treatment cost, increasing waste water discharge, increasing production cost, etc. The effect of reducing the amount of liquid discharge
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] Embodiments 1 to 5 are specific implementations of the silk interwoven jacquard fabric dyeing process of the present invention. Wherein embodiment 1 is the best embodiment. All LANASOL dyes used in Examples and Comparative Examples were produced by Huntsman. The HE type dyes used in the present invention are all produced by Taiwan Yongguang Chemical Industry Co., Ltd. The pretreatment methods in the examples and comparative examples are existing conventional pretreatment methods.
[0027] Example 1
[0028] In the present embodiment, the silk interwoven jacquard fabric that adopts silk fiber and cotton fiber jacquard to be interwoven is dyed into blue flash orange, and its method is as follows:
[0029] 1) Dyeing and color fixation: put the pretreated silk interwoven jacquard fabric into the prepared dye solution, and use the jigger dyeing method for dyeing. The dyeing temperature is kept at 80°C, and the dyeing time is 120 minutes; until the end of the total dyeing...
Embodiment 2
[0037] In the present embodiment, the silk interwoven jacquard fabric that adopts silk fiber and cotton fiber jacquard to be interwoven is dyed into scarlet flashing gold, and its method is as follows:
[0038] 1) Dyeing and color fixation: Put the pretreated silk interwoven jacquard fabric into the prepared dyeing solution, and use the jigger dyeing method for dyeing. The dyeing temperature is kept at 85°C, and the dyeing time is 80 minutes; until the end of the total dyeing time, discharge Waste liquid;
[0039] The preparation method of the dyeing solution is: 2.0% owf of Lanersol dye, 4% owf of HE dye, 50g / L of sodium sulfate, 8g / L of sodium carbonate and water; this formula can make silk fiber dye bright red, Cotton fibers are dyed gold;
[0040] 2) One wash with water: add water to raise the temperature to 60°C, wash the silk interwoven jacquard fabric, discharge the waste liquid after the end, and repeat the above steps twice;
[0041] 3) Soaping: Clean the silk inter...
Embodiment 3
[0046] In the present embodiment, the silk viscose interwoven jacquard fabric that adopts silk fiber and viscose fiber jacquard to be interwoven is dyed into green flash beige, and its method is as follows:
[0047] 1) Dyeing and color fixation: Put the pretreated silk interwoven jacquard fabric into the prepared dyeing solution, and use the jigger dyeing method for dyeing. The dyeing temperature is kept at 80°C, and the dyeing time is 100 minutes; until the total dyeing time is over, discharge Waste liquid;
[0048] The preparation method of the dyeing solution is: 2.50% owf of Lanersol dye, 0.05% owf of HE dye, 60g / L of sodium sulfate, 6g / L of sodium carbonate and water; this formula can make the silk fiber dyed green and sticky. The rubber fibers are dyed beige;
[0049] 2) One wash with water: add water to raise the temperature to 60°C, clean the silk viscose interwoven jacquard fabric, discharge the waste liquid after the end, and repeat the above steps twice;
[0050] ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com