A technology of LED packaging and detection method, which is applied in the direction of liquid tightness measurement using liquid/vacuum degree, and detecting the appearance of fluid at the leakage point, etc., which can solve the problems of expensive instrument cost, time-consuming and power consumption, and achieve the detection cycle The effect of shortening, simple material and good sealing
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0046] A method for detecting the airtightness of an LED encapsulant, comprising the steps of:
[0047] (1) Mix A and B glues according to the weight ratio, the weight ratio of the A glue and B glue is 1:1, stir for 4 to 12 minutes, so that the A and B glues are evenly mixed;
[0048](2) Defoaming: Put the well-mixed glue in a vacuum drying oven for 5 to 12 minutes to defoam, and the vacuum degree of the vacuum drying oven is -0.09~-0.1MPa;
[0049] (3) Glue filling: the base material (LED lamp beads or lamp holders) should be thoroughly cleaned and dried at 140°C before glue filling. Use a disposable toothpick to dip an appropriate amount of glue on the lamp beads according to the size of the lamp beads. Automatic leveling, observe the amount of dispensing obliquely, and the level with the upper concave surface of the lamp bead is the standard;
[0050] (4) Heating: Put the glue-filled lamp beads on a horizontal heat-resistant object, and then heat them in an oven at 100°C f...
Embodiment 2
[0054] A method for detecting the airtightness of an LED encapsulant, comprising the steps of:
[0055] (1) Mix the A and B glues according to the weight ratio, the weight ratio of the A glue and the B glue is 1:4, stir for 4 to 12 minutes, so that the A and B glues are evenly mixed;
[0056] (2) Defoaming: Heat the uniformly mixed glue to 45°C and keep it for 5 minutes, then put it in a vacuum drying oven for 5 to 12 minutes to defoam, the vacuum degree of the vacuum drying oven is -0.09~-0.1MPa);
[0057] (3) Glue filling: the base material (LED lamp beads or lamp holders) should be thoroughly cleaned and dried at 160°C before glue filling. Use a disposable toothpick to dip an appropriate amount of glue on the lamp beads according to the size of the lamp beads. Automatic leveling, observe the amount of dispensing obliquely, and the level with the upper concave surface of the lamp bead is the standard;
[0058] (4) Heating: Put the glue-filled lamp beads on a horizontal heat...
Embodiment 3
[0062] A method for detecting the airtightness of an LED encapsulant, comprising the steps of:
[0063] (1) Mix A and B glues according to the weight ratio, the weight ratio of the A glue and B glue is 1:2, stir for 4 to 12 minutes, so that the A and B glues are evenly mixed;
[0064] (2) Defoaming: Heat the uniformly mixed glue to 55°C and keep it for 1 minute, then place it in a vacuum drying oven for 5 to 12 minutes to defoam, the vacuum degree of the vacuum drying oven is -0.09~-0.1MPa;
[0065] (3) Glue filling: the base material (LED lamp beads or lamp holders) should be thoroughly cleaned and dried at 150°C before glue filling. Use a disposable toothpick to dip an appropriate amount of glue on the lamp beads according to the size of the lamp beads. Automatic leveling, observe the amount of dispensing obliquely, and the level with the upper concave surface of the lamp bead is the standard;
[0066] (4) Heating: Put the glue-filled lamp beads on a horizontal heat-resista...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com