Composite beneficiation reagent for extracting vanadium from stone coal

A kind of beneficiation agent and stone coal technology, applied in flotation, solid separation, etc., can solve the problems of not improving the comprehensive utilization value of stone coal resources, reducing the economic benefits of stone coal resource utilization, and not considering the utilization of carbon resources, etc., to achieve improvement Concentrate grade and recovery rate of vanadium, shorten flotation time, reduce the effect of dosing point

Active Publication Date: 2015-02-04
GUIZHOU BRANCH CHINA ALUMINUM IND
View PDF3 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, because the carbon in stone coal is hydrophobic and easy to float, the loss of carbon in the flotation process is serious, and at the same time, some vanadium minerals are also carried out, which reduces the economic benefits of stone coal resource utilization.
Ammonium salt vanadium separation, although this method can enrich the vanadium resources in stone coal and reduce the economic cost of vanadium extraction, but because the utilization of carbon resources in stone coal is not considered, it is difficult to regenerate the carbon in stone coal. Therefore, the comprehensive utilization value of stone coal resources has not been improved

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Composite beneficiation reagent for extracting vanadium from stone coal
  • Composite beneficiation reagent for extracting vanadium from stone coal

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0030] The compound beneficiation reagent for vanadium extraction from stone coal provided in this example is composed of the following components: 5g diesel oil, 0.5g benzyltriethylammonium chloride, 2g terpineol oil, 1g Tween-60, and 200g water.

[0031] The preparation method of the stone coal vanadium extraction compound mineral processing agent provided in this example: weigh 5g of diesel oil and 2g of terpineol oil, mix and stir the two evenly to obtain mixed solution E; weigh 0.5g of benzyltriethyl chloride Add ammonium and 1g Tween-60, add 200g water, stir and dissolve to make a mixed solution F; add the mixed solution E to the mixed solution F while stirring, and stir for 10 minutes to make a uniform emulsion.

Embodiment 2

[0033] The compound beneficiation agent for vanadium extraction from stone coal provided in this example is composed of the following components: 7g diesel oil, 0.3g dodecylamine hydrochloride, 1.5g MIBC, 4g OP-10, and 300g water.

[0034] The preparation method of the stone coal vanadium extraction composite mineral processing agent provided in this example: weigh 7g of diesel oil and 1.5g of MIBC, mix and stir them evenly to obtain mixed solution E; weigh 0.3g and 4g of dodecylamine hydrochloride For OP-10, add 300g of water, stir and dissolve to make a mixed solution F; add the mixed solution E to the mixed solution F while stirring, and stir for 30 minutes to make a uniform emulsion.

Embodiment 3

[0036] The compound beneficiation reagent for extracting vanadium from stone coal provided in this embodiment is composed of the following components: 5g kerosene, 2g dodecyltrimethylammonium chloride, 1g terpineol oil, 2g sodium dodecylsulfonate, 250g water .

[0037] The preparation method of the stone coal vanadium extraction composite mineral processing agent provided in this example: weigh 5g of kerosene and 1g of terpineol oil, mix and stir the two evenly, and prepare mixed solution E; weigh 2g of dodecyl trimethyl chloride Add ammonium chloride and 2g of sodium dodecylsulfonate, add 250g of water, stir and dissolve to make a mixed solution F; add the mixed solution E to the mixed solution F while stirring, and stir for 20 minutes to make a uniform emulsion.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to a composite beneficiation reagent for extracting vanadium from stone coal. The composite beneficiation reagent for extracting the vanadium from the stone coal is characterized in that the composite beneficiation reagent is composed of a component A, a component B, a component C, a component D and water, the component A is kerosene and / or diesel oil, the component B is quaternary ammonium salt class matter and / or aliphatic amine hydrochloride class matter, the component C is any one or more of alcohol ranging from C4 to C8, 4-methyl-cyclohexyl-methanol, MIBC, terpenic oil, methyl triisopropoxy silane, and the component D is any one or more of alkyl-sulfonate ranging from C8 to C12, OP-10 and Tween-60. The composite beneficiation reagent for extracting the vanadium from the stone coal is prepared by a plurality of components according to a certain proportion and a rule, combination of the components of the reagent can be adjusted according to different mineral properties so that a series of flotation reagents can be prepared, and thebest use effect is achieved.

Description

technical field [0001] A compound beneficiation agent for vanadium extraction from stone coal. It relates to a composite mineral dressing agent for extracting vanadium from stone coal. Background technique [0002] Stone coal is a polymetallic paragenetic ore with low carbon content, low calorific value and low grade. The calorific value of stone coal is not high, generally around 800 kcal / kg, and it is a low calorific value fuel. More than 60 kinds of associated elements have been found in my country's stone coal resources, among which vanadium is the main one that can form industrial deposits, followed by molybdenum, uranium, phosphorus, silver and so on. [0003] my country is rich in stone coal resources. How to study and extract vanadium and other associated elements while making full use of the low calorific value energy of stone coal can not only improve the utilization value of stone coal, but also provide more urgently needed metal materials for my country's natio...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): B03D1/018B03D1/04B03D101/02
Inventor 李旺兴陈湘清刘万超李素敏马俊伟陈占华田应忠李莎莎李花霞郭鑫
Owner GUIZHOU BRANCH CHINA ALUMINUM IND
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products