Water-lubricated wear-resistant cooling liquid and preparation method thereof
A cooling fluid and water lubrication technology, applied in lubricating compositions, petroleum industry, etc., can solve the problems of limited application of water-based metalworking fluids, poor lubricity and corrosion resistance, unstable chemical properties, etc., to improve occupational health. , Good chemical corrosion resistance and obvious lubricating effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032]The water-lubricated wear-resistant coolant consists of the following percentage components in parts by weight:
[0033] Water 89.5g
[0034] HM-55 Closed System High Temperature Antirust Liquid 8.5g
[0035] Carbon nanotubes 0.2g
[0036] Graphite 1.8g
[0037] The preparation method of water-lubricated wear-resistant coolant: use 89.5g of water as the main raw material, add 0.2g of carbon nanotubes, 8.5g of HM-55 closed system high-temperature resistant anti-rust liquid, and 1.8g of graphite, and stir at high speed with the equipped stirring equipment Ready in 30 minutes.
Embodiment 2
[0039] The water-lubricated wear-resistant coolant consists of the following percentage components in parts by weight:
[0040] Water 87.5g
[0041] VpCI-377 high temperature antirust liquid 10g
[0042] n-Cu 0.5g
[0043] Graphite 2g
[0044] The preparation method of water-lubricated wear-resistant coolant: use 87.5g of water as the main raw material, add n-Cu 0.5g, VpCI-377 high temperature resistant anti-rust liquid 10g, graphite 2g, and stir at high speed for 30 minutes with the equipped stirring equipment Prepared.
Embodiment 3
[0046] The water-lubricated wear-resistant coolant consists of the following percentage components in parts by weight:
[0047] Water 81.9g
[0048] 787B Closed System Cooling Water Antirust Liquid 15g
[0049] n-Ph 1g
[0050] Graphite 2.1g
[0051] The preparation method of water-lubricated wear-resistant coolant: use 81.9g water as the main raw material, add n-Ph 1g, 787B closed system cooling water anti-rust liquid 15, graphite 2.1g, and stir for 30 minutes at high speed with the equipped stirring equipment Prepared.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology