A technology of water-based multi-color coatings and multi-color coatings, applied in multi-color effect coatings, anti-fouling/underwater coatings, coatings, etc., can solve the problems of poor storage stability, harsh production conditions, and cumbersome production processes of multi-color coatings, and achieve rich Decoration and protection needs, easy construction, and stable product quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0042] An environment-friendly water-based colorful paint, the raw material formula includes A component, B component and C component:
[0043] A component is a composite granulated colloidal solution, including components by mass: 3-14 parts of montmorillonite; 0-1.0 parts of sodium hexametaphosphate; 0-1.2 parts of sodium pyrophosphate pentahydrate; 0-1.0 parts of pH regulator; 86-97 parts of water;
[0044] Component B is the base paint for granulation, including components by mass: 20-80 parts of water; 8-15 parts of granulation colloidal solution; 0.1-0.5 parts of defoaming agent; 2-40 parts of pigments and fillers; 0.6-1.5 parts of composite coupling resin; 0.05-0.2 parts of preservative; 0.05-0.15 parts of PH regulator; 2-30 parts of elastic self-crosslinking emulsion. The composite coupling resin is a mixture of 4 parts of hydroxyethyl propyl cellulose and 1 part of styrene maleic anhydride copolymer.
[0045] Component C is paint-forming emulsion, including componen...
Embodiment 2
[0047] A preparation method of an environment-friendly water-based colorful paint, the preparation process comprising the following steps:
[0048] The first step: preparation of compound granulation colloidal solution
[0049] According to the mass ratio, 3-14 parts of montmorillonite, 0-1 part of sodium hexametaphosphate, 0-1.2 parts of sodium pyrophosphate pentahydrate, mix and add to 86-97 parts of water to disperse, add ammonia water to adjust pH8.5-9.5 , to obtain A component.
[0050] The second step: the preparation of each color particle
[0051] (1) Preparation of white base paint
[0052]According to mass ratio, 20-80 parts of water; 0.1-0.5 parts of defoamer; 0.1-0.5 parts of anionic and nonionic wetting and dispersing agent; 0.2 parts; 0.05-0.15 parts of PH regulator; 2-30 parts of elastic self-crosslinking emulsion; agent, anionic non-ionic wetting and dispersing agent, pigment and filler, composite coupling resin, disperse for 10-40min, add preservative, ela...
Embodiment 3
[0063] A preparation method of an environment-friendly water-based colorful paint, the preparation process comprising the following steps:
[0064] 1. Preparation of compound granulation colloidal solution
[0065] Weigh 8 parts of montmorillonite, 0.3 part of sodium hexametaphosphate, and 0.2 part of sodium pyrophosphate pentahydrate according to the weight ratio, mix them well, slowly add them to 91 parts of water to disperse evenly, add 0.5 parts of ammonia water to adjust the pH to 8.5~9.5, and obtain A component.
[0066] 2. Preparation of each color particle
[0067] (1) Preparation of white base paint
[0068] Weigh 46 parts of water by weight, 0.2 parts of defoamer NXZ, 0.2 parts of anionic nonionic wetting and dispersing agent 4010, 1 part of rutile titanium dioxide, 16 parts of 4000 mesh calcined kaolin, 1.4 parts of RX-15, 0.1 part of LFM, 0.1 part of ammonia water, 25 parts of elastic self-crosslinking emulsion 8238; 10 parts of component A; start the disperse...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com