No-shrinkage grouting filler with adjustable performance
A grouting material, non-shrinkage technology, applied in the field of basic engineering grouting material and non-shrinkage grouting material, can solve the problems of grouting material not filling the entire space, loose equipment base, insufficient fluidity, etc., achieving low brittleness and low price. , the effect of good liquidity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0034] Embodiment 1, a kind of performance-adjustable non-shrinkage grouting material,
[0035] The grouting material is composed of cementitious material, quartz sand and a small amount of water reducer, expansion agent, water loss reducer, anti-early settlement agent, anti-early shrinkage agent and mixing water. The ratio of various materials is:
[0036] PO42.5R type cement 40.5%;
[0037] Fly ash 6.1%;
[0038] Quartz sand 49%;
[0039] The gradation of quartz sand is:
[0040] 0.0~0.16mm 9% (by weight)
[0041] 0.16~0.315mm 35% (weight ratio)
[0042] 0.315~1.25mm 28% (weight ratio)
[0043] 1.25~2.5mm 18% (weight ratio)
[0044] 2.5~3.0mm 10% (weight ratio)
[0045] Naphthalenesulfonate formaldehyde condensate and sulfamate mixture 1.28%, the ratio of naphthalenesulfonate formaldehyde condensate and sulfamate is: 3:1.
[0046] Burnt quicklime and sulphoaluminate expansion agent 3.0%, the ratio of burnt quicklime and sulphoaluminate expansion agent is: 1:6
[004...
Embodiment 2
[0052] Example 2, a non-shrinkage grouting material with adjustable performance
[0053] The grouting material is composed of cementitious material, quartz sand and a small amount of water reducer, expansion agent, water loss reducer, anti-early settlement agent, anti-early shrinkage agent and mixing water. The ratio of various materials is:
[0054] PO42.5R type cement, 41.5%.
[0055] Fly ash, 7.4%.
[0056] Quartz sand, 47.5%.
[0057] The gradation of quartz sand is:
[0058] 0.0~0.16mm 8% (by weight)
[0059] 0.16~0.315mm 35% (weight ratio)
[0060] 0.315~1.25mm 30% (weight ratio)
[0061] 1.25~2.5mm 15% (weight ratio)
[0062] 2.5~3.0mm 12% (weight ratio)
[0063] Naphthalenesulfonate formaldehyde condensate and sulfamate mixture, 0.95%. (The ratio of naphthalenesulfonate formaldehyde condensate and sulfamate is: 3:1).
[0064] Burnt quicklime and sulphoaluminate expansion agent, 2.58%. (The ratio of overburned quicklime and sulphoaluminate expansion agent expans...
Embodiment 3
[0070] Embodiment 3, a kind of non-shrinkage grouting material with adjustable performance
[0071] The grouting material is composed of cementitious material, quartz sand and a small amount of water reducing agent, expansion agent, water loss reducing agent, anti-early settlement agent, anti-early shrinkage agent and mixing water. The ratio of various materials is:
[0072] PO42.5R type cement, 31.5%.
[0073] Ultrafine silica fume powder, 1.2%.
[0074] Fly Ash, 10%
[0075] Quartz sand, 54.3%.
[0076] The gradation of quartz sand is:
[0077] 0.0~0.16mm 8% (by weight)
[0078] 0.16~0.315mm 34% (weight ratio)
[0079] 0.315~1.25mm 29% (weight ratio)
[0080] 1.25~2.5mm 20% (weight ratio)
[0081] 2.5~3.0mm 9% (weight ratio)
[0082] Naphthalenesulfonate formaldehyde condensate, 1.0%.
[0083] Burnt quicklime and sulphoaluminate expansion agent, 1.83%. (The ratio of burnt quicklime and sulphoaluminate expansion agent is: 1:4.5)
[...
PUM
Property | Measurement | Unit |
---|---|---|
length | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.