A ZIF-8, film-forming technology, applied in separation methods, chemical instruments and methods, membranes, etc., can solve the problems of difficult to synthesize thin and continuous dense, swelling, poor stability, low membrane strength, etc., and achieve good gas separation performance. and the effects of increased flux, improved mechanical strength, and simple preparation process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0045] (1) Pretreatment α-Al 2 o 3 Carrier tube: the outer diameter of the tube is 12mm, the inner diameter of the tube is 8mm, the average pore diameter is 2-5μm, and the porosity is about 30-40%; the outer surface of the carrier tube is polished with 800 mesh and 1500 mesh sandpaper; it is removed by ultrasonic vibration with deionized water Residual particles on the carrier tube, repeat several times until the water used to wash the tube is no longer turbid, then use acid and alkali ultrasonic vibration to remove the residue in the carrier hole, and wash with deionized water until neutral; finally the tube Put it in an oven to dry, then place it in a muffle furnace for calcination at 550°C for 6 hours, and seal both ends for later use;
[0046] (2) Zinc acetate (ZnAc 2 ) into 100ml of ethylene glycol methyl ether, and stirred in a constant temperature water bath at 70°C to obtain a milky white suspension; then slowly add 5ml of ethanolamine to the suspension of zinc aceta...
Embodiment 2
[0051] (1) Pretreatment α-Al 2 o 3 Carrier tube: the outer diameter of the tube is 12mm, the inner diameter of the tube is 8mm, the average pore diameter is 2-5μm, and the porosity is about 30-40%; the outer surface of the carrier tube is polished with 800 mesh and 1500 mesh sandpaper; it is removed by ultrasonic vibration with deionized water Residual particles on the carrier tube, repeat several times until the water used to wash the tube is no longer turbid, then use acid and alkali ultrasonic vibration to remove the residue in the carrier hole, and wash with deionized water until neutral; finally the tube Put it in an oven to dry, then place it in a muffle furnace for calcination at 550°C for 6 hours, and seal both ends for later use;
[0052] (2) Zinc acetate (ZnAc 2 ) into 100ml of ethylene glycol methyl ether, and stirred in a constant temperature water bath at 70°C to obtain a milky white suspension; then slowly add 5ml of ethanolamine to the suspension of zinc aceta...
Embodiment 3
[0057] The gas phase filling synthesis ZIF-8 film prepared by example 1 is carried out single-component gas and pressure test, test result is as attached Figure 7 Film formation curve in the hole. After testing, H 2 The permeate flux range is 4.58×10 -7 mole m -2 ·s -1 pa -1 , H 2 / CH 4 , the separation factor is 13, which is far greater than Knudsen diffusion, which proves the feasibility of this method and has a certain separation ability for gases; when the pressure is increased, H 2 / CH 4 The separation factor remained basically stable, indicating strong applicability.
PUM
Property | Measurement | Unit |
---|---|---|
pore size | aaaaa | aaaaa |
pore size | aaaaa | aaaaa |
porosity | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com