An environmentally friendly paint and low odor technology, applied in the coating and other directions, can solve the problems of human harm, paint easily emits odor, volatile and other problems, and achieves the effect of improving environmental protection performance, beautiful appearance and high transparency.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0045] A low-odor environment-friendly paint for furniture, comprising the following components in parts by mass:
[0046] 67.5 parts of butyl acetate; 19.5 parts of n-butanol; 10.5 parts of isopropanol; 30 parts of polyacrylic acid-based adsorption resin; 9 parts of xylene.
[0047] In this embodiment, the polyacrylic acid-based adsorption resin is polymethacrylic acid.
[0048] The paint is prepared as follows:
[0049] (1) In a 200L reactor, under normal temperature conditions, add 67.5kg of butyl acetate, 19.5kg of n-butanol, 10.5kg of isopropanol, and 9kg of xylene, and stir at a speed of 40r / min;
[0050] (2) Add polymethacrylic acid 30kg while stirring;
[0051](3) After stirring and mixing evenly, the paint is obtained.
Embodiment 2
[0053] A low-odor environment-friendly paint for furniture, comprising the following components in parts by mass:
[0054] 79 parts of butyl acetate; 23 parts of n-butanol; 12.3 parts of isopropanol; 35 parts of polyacrylic acid-based adsorption resin; 10.5 parts of xylene.
[0055] In this embodiment, the polyacrylic acid-based adsorption resin is poly(2-ethylacrylic acid).
[0056] The paint is prepared as follows:
[0057] (1) In a 200L reactor, under normal temperature conditions, add 79kg of butyl acetate, 23kg of n-butanol, 12.3kg of isopropanol, and 10.5kg of xylene, and stir at a speed of 40r / min;
[0058] (2) Add poly(2-ethylacrylic acid) 35kg while stirring;
[0059] (3) After stirring and mixing evenly, the paint is obtained.
Embodiment 3
[0061] A low-odor environment-friendly paint for furniture, comprising the following components in parts by mass:
[0062] 90 parts of butyl acetate; 26 parts of n-butanol; 14 parts of isopropanol; 40 parts of polyacrylic acid-based adsorption resin; 12 parts of xylene.
[0063] In this embodiment, the polyacrylic acid-based adsorption resin is poly(2-propylacrylic acid).
[0064] The paint is prepared as follows:
[0065] (1) In a 200L reactor, under normal temperature conditions, add 90kg of butyl acetate, 26kg of n-butanol, 14kg of isopropanol, and 12kg of xylene, and stir at a speed of 40r / min;
[0066] (2) Add poly(2-propylacrylic acid) 40kg while stirring;
[0067] (3) After stirring and mixing evenly, the paint is obtained.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com