Stably-colored silicon dioxide particles and preparation method thereof
A technology of silica and color stability, applied in chemical instruments and methods, cosmetic preparations, preparations for skin care, etc., can solve the problems of fading, easy discoloration, color bleeding, etc., and achieves low production cost, simple preparation method, Stable performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] Embodiment 1, coloring stable colored silica particle of the present invention and its preparation
[0029] The first step: inject 2m sulfuric acid solution with a concentration of 0.4M into the reactor 3 , then add 0.4L of hydroxyl silicone oil, stir and activate for 10min;
[0030] Step 2: Add a water glass solution with a modulus of 3.3 and a concentration of 0.4M to the reaction kettle for reaction. When the pH value of the system is 3, add 2L of Edible Blue No. 1, and stop adding when the pH value of the system is 6 Water glass solution, continue to stir until the material system is transformed into a gel;
[0031] Step 3: Press-filter the formed silica gel, wash the gel filter cake with water to remove salt and residual reaction aids, dry and pulverize the washed gel filter cake to obtain silica particles;
[0032] The fourth step: put 5 kg of silicon dioxide particles into the reaction tank, add 20 kg of allyl alcohol polyoxyalkyl ether aqueous solution with a ...
Embodiment 2
[0033] Example 2, Colored and stable colored silica particles of the present invention and their preparation
[0034] The first step: inject 3m sulfuric acid solution with a concentration of 0.6M into the reactor 3 , then add 1.8L of hydroxy silicone oil, stir and activate for 15min;
[0035]Step 2: Add a water glass solution with a modulus of 3.3 and a concentration of 0.8M to the reactor for reaction. When the pH value of the system is 4, add edible red No. 3 9L, and stop adding water when the pH value of the system is 7. Glass solution, continue to stir until the material system turns into a gel;
[0036] Step 3: Press-filter the formed silica gel, wash the gel filter cake with water to remove salt and residual reaction aids, dry and pulverize the washed gel filter cake to obtain silica particles;
[0037] The fourth step: put 5 kg of silicon dioxide particles into the reaction tank, add 30 kg of allyl alcohol polyoxyalkyl ether aqueous solution with a mass percentage con...
Embodiment 3
[0038] Example 3, Colored and stable colored silica particles of the present invention and their preparation
[0039] The first step: inject 2m sulfuric acid solution with a concentration of 0.8M into the reactor 3 , then add 0.8L of hydroxyl silicone oil, stir and activate for 15min;
[0040] Step 2: Add a water glass solution with a modulus of 3.3 and a concentration of 0.6M to the reactor for reaction. When the pH value of the system is 4, add edible yellow No. 5 4L, and stop adding water when the pH value of the system is 6. Glass solution, continue to stir until the material system turns into a gel;
[0041] Step 3: Press-filter the formed silica gel, wash the gel filter cake with water to remove salt and residual reaction aids, dry and pulverize the washed gel filter cake to obtain silica particles;
[0042] The fourth step: put 5 kg of silicon dioxide particles into the reaction tank, add 25 kg of allyl alcohol polyoxyalkyl ether aqueous solution with a concentration ...
PUM
Property | Measurement | Unit |
---|---|---|
modulus | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction