Heat sensitive paper top coating paint, heat sensitive paper paint and heat sensitive paper
A surface coating and coating technology, applied in the thermal paper surface coating coating, thermal paper coating and thermal paper fields, can solve the problems of reducing the service life of thermal printers, print head damage, etc., to improve the service life, The effect of reducing accumulation and reducing damage
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] A. Provide the original base paper;
[0028] B. Preparation of heat-sensitive paper primer coating solution: under high-speed stirring conditions, mix 82g of light calcium carbonate, plastic pigment and silicon dioxide with a mass ratio of 2:2:1, 18g of polyvinyl alcohol, and 257g of water Mix evenly, thereby the quality that obtains primer coating accounts for the primer coating solution that the total mass of primer coating solution is 28%;
[0029] C. Using a coating machine, apply 7.2g / m on the surface of base paper 2 The coating amount of the primer coating solution is applied, and the primer layer is formed after drying;
[0030] D. Preparation of heat-sensitive paper surface coating solution: (1) Preparation of the first mixed solution: 40 g of 2,4 diphenylsulfone phenol, 4.5 g of polyvinyl alcohol, and 67 g of water are mixed to prepare the first mixed solution with a mass fraction of 40%. A mixed solution, and then ground in a wet grinder until the solid part...
Embodiment 2
[0033] A. Provide the original base paper;
[0034] B. Preparation of heat-sensitive paper primer coating solution: under high-speed stirring conditions, mix 90 g of a mixture of calcined kaolin and plastic pigments with a mass ratio of 1:1, 10 g of polyvinyl alcohol, and 213 g of water to obtain a primer layer The quality of the paint accounts for the primer coating solution that is 32% of the total mass of the primer coating solution;
[0035] C. Using a coating machine, apply 8.0g / m on the surface of base paper 2 The coating amount of the primer coating solution is applied, and the primer layer is formed after drying;
[0036] D. Preparation of heat-sensitive paper surface coating solution: (1) Preparation of the first mixed solution: 36g of 4,4 diphenylsulfone phenol, 3.5g of polyvinyl alcohol, and 55g of water were mixed to prepare the first mixed solution with a mass fraction of 42%. A mixed solution, then grind in a wet grinder until the solid particle size in the fir...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com