Preservative treatment method for decorative timber
A treatment method and wood preservative technology, applied in wood treatment, pressurized wood treatment, wood treatment details, etc., can solve problems such as poor wood preservative effect, preservatives cannot enter cells, etc., and achieve the effect of improving preservative effect.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0025] The preservative treatment method of decorative wood includes the following steps;
[0026] S1. Put the dry wood in a closed container;
[0027] S2. Use a high-pressure pump to pressurize the closed container to make the pressure in the container 5Mpa for 60 minutes;
[0028] S3. Take the wood out of the airtight container and place it in a dry and ventilated environment for no less than 7 days;
[0029] S4. Put the dried wood in the airtight container again, and vacuumize so that the pressure in the airtight container is -0.05Mpa and the duration is 10 minutes;
[0030] S5. After filling the airtight container with water-soluble preservative, pressurize the airtight container to 1Mpa and keep it for 20 minutes; decompress the airtight container so that the pressure in the airtight container is 0.5Mpa and keep it for 10 minutes; The container is pressurized so that the pressure in the airtight container is 2Mpa and kept for 20 minutes; the airtight container is decompressed so t...
Embodiment 2
[0036] The preservative treatment method of decorative wood includes the following steps;
[0037] S1. Put the dry wood in a closed container;
[0038] S2. Use a high-pressure pump to pressurize the closed container so that the pressure inside the container is 10Mpa for 60 minutes;
[0039] S3. Take the wood out of the airtight container and place it in a dry and ventilated environment for no less than 7 days;
[0040] S4. Put the dried wood into the airtight container again, and vacuumize so that the pressure in the airtight container is -0.1Mpa and the duration is 130 minutes;
[0041] S5. After filling the airtight container with water-soluble preservative, pressurize the airtight container to 3Mpa and keep it for 40 minutes; depressurize the airtight container so that the pressure in the airtight container is 1Mpa and keep it for 20 minutes; for the airtight container Pressurize so that the pressure in the airtight container is 4Mpa and keep it for 40 minutes; depressurize the airt...
Embodiment 3
[0047] The preservative treatment method of decorative wood includes the following steps;
[0048] S1. Put the dry wood in a closed container;
[0049] S2. Use a high-pressure pump to pressurize the closed container so that the pressure in the container is 6Mpa for 60 minutes;
[0050] S3. Take the wood out of the airtight container and place it in a dry and ventilated environment for no less than 7 days;
[0051] S4. Put the dried wood in the airtight container again, and vacuum, so that the pressure in the airtight container is -0.08Mpa and the duration is 20 minutes;
[0052] S5. After filling the airtight container with water-soluble preservative, pressurize the airtight container to 2Mpa and keep it for 30 minutes; depressurize the airtight container so that the pressure in the airtight container is 0.8Mpa and keep it for 15 minutes; The container is pressurized so that the pressure in the airtight container is 3Mpa and kept for 30 minutes; the airtight container is decompressed s...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com