Concrete block and manufacturing method thereof
A technology for a concrete block and a manufacturing method, applied in the field of building materials, can solve the problems of reducing infiltration channels, economic losses, waste of resources, etc., and achieve the effects of improving strength and stability, improving defoaming rate, and good dispersibility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] A kind of concrete block manufacture method: this method at first adds cocoic acid diethanolamide, n-octanol, behenyl palmitate, and hydroxyl silicone oil into a pressurizable container, and the pressure of the pressurizable container is controlled at 0.18MPa, the temperature is controlled at 53°C, and the pressure is maintained for 15 minutes. After the pressure is maintained, the pressure is released and the temperature is lowered to normal pressure and temperature, and the temperature is 38-42°C. Magnetic stirring, coconut acid diethanolamide , n-octanol, behenyl palmitate, the molar ratio of hydroxy silicone oil and Span 80 is 1:2.5:1.5:12:0.3, the magnetic stirring speed is 180r / min, stir at constant temperature for 30min, and then add polyoxygen Propylene glyceryl ether is mixed evenly and naturally cooled to room temperature to obtain a defoamer,
[0020] After that, waste asphalt will be selected for crushing, broken into 5-15mm particles, washed with water, air...
Embodiment 2
[0024] A kind of concrete block manufacture method: this method at first adds cocoic acid diethanolamide, n-octanol, behenyl palmitate, and hydroxyl silicone oil into a pressurizable container, and the pressure of the pressurizable container is controlled at 0.2MPa, the temperature is controlled at 55°C, and the pressure is maintained for 20 minutes. After the pressure is maintained, the pressure is released and the temperature is lowered to normal pressure and temperature, and the temperature is 38-42°C. Magnetic stirring, coconut acid diethanolamide , n-octanol, behenyl palmitate, the molar ratio of hydroxy silicone oil and Span 80 is 1:3:1.8:14:0.4, the magnetic stirring speed is 190r / min, stir at constant temperature for 30min, and then add polyoxygen Propylene glyceryl ether was mixed evenly and naturally cooled to room temperature to obtain a defoamer.
[0025] After that, waste asphalt will be selected for crushing, broken into 5-15mm particles, washed with water, aired...
Embodiment 3
[0029] A method for manufacturing a concrete block: the method firstly mixes coconut acid diethanolamide, n-octanol, behenyl palmitate, and hydroxyl silicone oil into a pressurizable container, and the pressure of the pressurizable container is controlled at 0.2MPa, the temperature is controlled at 54°C, and the pressure is maintained for 16 minutes. After the pressure is maintained, the pressure is released and the temperature is lowered to normal pressure and temperature, and the temperature is 42°C. Magnetic stirring, coconut acid diethanolamide, normal The molar ratio of octanol, behenyl palmitate, hydroxyl silicone oil and Span 80 is 1:3.5:1.5:14:0.5, the magnetic stirring speed is 160r / min, stirring at constant temperature for 30min, and then adding polyoxypropylene glycerin The ether was mixed evenly and cooled naturally to room temperature to obtain a defoamer.
[0030] Afterwards, waste asphalt will be selected for crushing, broken into 5-15mm particles, washed with w...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com