A kind of silver-containing antibacterial fabric coating glue and preparation and use method thereof
A technology of antibacterial fabric and coating glue, which is applied in the fields of antibacterial coating glue and its preparation, silver-containing antibacterial fabric coating glue and its preparation, and can solve the problems of large particle size, wide distribution range and easy agglomeration of antibacterial agents , to achieve the effect of overcoming easy agglomeration, long-lasting antibacterial performance, and overcoming easy discoloration
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] The formulation of the coating glue that doctors take for work is shown in Table 1
[0029] raw material
[0030] Dissolve the dried coating glue in acetic acid, use the applicator to evenly apply a certain concentration of coating glue / acetic acid solution to the fabric, and dry it to evaporate the solvent or water, thereby forming a continuous film on the surface of the fabric , to prepare antibacterial coated fabrics.
Embodiment 2
[0032] The formula of coating glue for fabric sofa is shown in Table 1
[0033] raw material
Embodiment 3
[0035] The coating glue formula for socks is shown in Table 1
[0036] raw material
parts by mass
Emulsion of acrylate and acrylamide copolymer
80
Silver loaded zirconium phosphate
10
Dispersant (polyphosphate)
3
Stabilizer (fumed silica)
3
solvent
20
[0037] The preparation method of silver-containing antibacterial fabric coating adhesive comprises the following steps:
[0038] (1) Add 70-80 parts of water-based acrylic emulsion and 10-20 parts of deionized water into the dispersion tank, stir at room temperature for 5-20 minutes, and the stirring speed is 200-500 rpm;
[0039] (2) Add dispersant and stabilizer at one time, stir at room temperature for 10-30 minutes, stirring speed 200-500 rpm;
[0040] (3) Add silver-loaded inorganic antibacterial agent (0.5-3µm), and oscillate ultrasonically for 30-60 minutes;
[0041] (4) After suction filtration, bake at 80-100°C for 2-3 hours to obtain the finished pr...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com