Antique matte cracked glaze and preparation technology thereof
A cracked glaze and matte technology, which is applied to clay products, other household utensils, household utensils, etc., can solve the problems of poor adaptability to rapid firing, unstable glaze effect, single glaze effect, etc., and achieve high social benefits and Economic benefits, stable glaze effect, and the effect of improving market competitiveness
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment approach 1
[0017] Antique matt crackle glaze, the preparation of the crackle glaze includes the following raw materials in parts by weight: 27 parts of feldspar, 42 parts of limestone, 8 parts of kaolin, 8 parts of calcined kaolin, and 15 parts of quartz.
[0018] The preparation of antique matte crackle glaze comprises the following steps:
[0019] a. Preparation of glaze: mix 27 parts of feldspar, 42 parts of limestone, 8 parts of kaolin, 8 parts of calcined kaolin, and 15 parts of quartz to make a mixture, and then add water according to the weight ratio of mixture: water = 1:0.80 , the crackle glaze was obtained after ball milling and sieving;
[0020] b. Glazing: apply crack glaze on the surface of the laterite porcelain body;
[0021] c. Firing: Send the glazed laterite porcelain body into a tunnel kiln for firing at a firing temperature of 1260°C and a firing time of 12 hours. After cooling out of the kiln, it will have a glazed surface with cracks and cracks. semi-finished prod...
Embodiment approach 2
[0025] Antique matt crackle glaze, the preparation of the crackle glaze includes the following raw materials in parts by weight: 27 parts of feldspar, 45 parts of limestone, 8 parts of kaolin, 8 parts of calcined kaolin, and 12 parts of quartz.
[0026] The preparation of antique matte crackle glaze comprises the following steps:
[0027] a. Preparation of glaze: Mix 27 parts of feldspar, 45 parts of limestone, 8 parts of kaolin, 8 parts of calcined kaolin, and 12 parts of quartz to make a mixture, and then add water according to the weight ratio of mixture: water = 1:0.75 , the crackle glaze was obtained after ball milling and sieving;
[0028] b. Glazing: apply crack glaze on the surface of the laterite porcelain body;
[0029] c. Firing: Send the glazed laterite porcelain body into a rotary electric kiln for firing. The firing temperature is 1250°C and the firing time is 24 hours. After cooling out of the kiln, there will be a glazed surface with cracks and cracks. semi-f...
Embodiment approach 3
[0032] Antique matt crackle glaze, the preparation of the crackle glaze includes the following raw materials in parts by weight: 30 parts of feldspar, 42 parts of limestone, 8 parts of kaolin, 8 parts of calcined kaolin, and 12 parts of quartz.
[0033] The preparation of antique matte crackle glaze comprises the following steps:
[0034] a. Preparation of glaze: mix 30 parts of feldspar, 42 parts of limestone, 8 parts of kaolin, 8 parts of calcined kaolin, and 12 parts of quartz to make a mixture, and then add water according to the weight ratio of mixture: water = 1:0.85 , the crackle glaze was obtained after ball milling and sieving;
[0035] b. Glazing: apply crack glaze on the surface of the laterite porcelain body;
[0036] c. Firing: Send the glazed laterite porcelain body into a rotary electric kiln for firing at a firing temperature of 1270°C and a firing time of 12 hours. After cooling out of the kiln, it will have a glazed surface with cracks and cracks. semi-fini...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com