Cigarette molding paper water paint containing tea extract
A technology of water-based paint and tea extract, applied in paper paint, coating, papermaking and other directions, can solve the problem that it is difficult for smokers to quit smoking, and achieve the effects of low cost, simple production process and safe smoking
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A water-based coating for cigarette forming paper containing tea extract, the raw material ratio is as follows: 100 kg of water, 20 kg of tea, 15 kg of carboxymethyl cellulose, 8 kg of tapioca starch, and 8 kg of guar gum.
[0023] Follow the steps below to produce:
[0024] A. Heat water to boiling, add crushed tea, steep for 0.5 hours, filter, and take filtrate a; and
[0025] B, carboxymethyl cellulose, tapioca starch, guar gum are mixed homogeneously; With
[0026] C. First heat the filtrate a obtained in the above step A to 80° C., and then stir and mix it with the mixture obtained in step B to prepare a water-based coating for forming paper.
Embodiment 2
[0028] A water-based coating for cigarette forming paper containing tea extract, the raw material ratio is as follows: water 100kg, tea 21kg, carboxymethyl cellulose 15kg, tapioca starch 9kg, guar gum 9kg
[0029] Follow the steps below to produce:
[0030] A. Heat the water to boiling, add crushed tea, soak for 0.75 hours, filter, and take the filtrate a; and
[0031] B, carboxymethyl cellulose, tapioca starch, guar gum are mixed homogeneously; With
[0032] C. First heat the filtrate a obtained in the above step A to 82° C., and then stir and mix it with the mixture obtained in step B to prepare a water-based coating for molding paper.
Embodiment 3
[0034] A water-based coating for cigarette forming paper containing tea extract, the raw material ratio is as follows: water 100kg, tea 22kg, carboxymethyl cellulose 17kg, tapioca starch 8kg, guar gum 10kg
[0035] Follow the steps below to produce:
[0036] A. Heat the water to boiling, add crushed tea, steep for 1 hour, filter, and take the filtrate a; and
[0037] B, carboxymethyl cellulose, tapioca starch, guar gum are mixed homogeneously; With
[0038] C. First heat the filtrate a obtained in the above step A to 85° C., and then stir and mix it with the mixture obtained in step B to prepare a water-based coating for forming paper.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com