A drying method and technology for wood, which are applied in wood drying, dryers for stationary materials, drying of solid materials, etc., can solve the problems of increasing the relative humidity of the drying environment and reducing the gradient of moisture content in the drying process of fast-growing wood.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0094] 1. Determination of the initial moisture content of the wood to be dried (M 0 )
[0095] According to the sampling inspection standard, randomly select a representative wood from the fast-growing eucalyptus wood to be dried, and first weigh its wet weight (G 湿 ), then place the weighed fast-growing wood in an oven with a temperature of (103±2)°C, dry it, and weigh it every 6 hours. When the weight difference between two consecutive weighings is less than 0.02g, it is considered as Dried to a dry state, the weight of the fast-growing wood at this time is the dry weight of the fast-growing wood (G 干 );
[0096] According to the wood moisture content formula (1), calculate the initial moisture content of the wood to be dried (M 0 ):
[0097]
[0098] The initial moisture content M of fast-growing timber eucalyptus wood in the embodiment of the present invention 0 It is 95% (60-200% of the initial moisture content of the wood to be dried is applicable to the present...
Embodiment 2
[0145] 1. Determination of the initial moisture content of the wood to be dried (M 0 )
[0146] Same as embodiment 1;
[0147] 2. Palletizing
[0148] Except that 5 temperature sensor groups are arranged at the drying medium inflow end and the outflow end of the material pile, all the other are the same as embodiment 1;
[0149] 3. Wood pretreatment
[0150] Except step A) in the pretreatment process: during the pretreatment process, measure the dry and wet bulb temperature T of the drying medium in the drying chamber every 2min (usually 1-3min) 干 and T 湿 ; Then when calculating the relative humidity (Φ) in the drying chamber according to the formula (3):
[0151] (A1) When Φ≤80%, open the steam generator in the drying chamber, spray steam into the drying kiln, and increase the relative humidity in the drying kiln;
[0152] (A2) When Φ≥90%, turn off the steam generator, stop spraying steam, and keep the relative humidity in the drying kiln higher than 80%, otherwise;
...
Embodiment 3
[0165] 1. Determination of the initial moisture content of the wood to be dried (M 0 )
[0166] Same as embodiment 1;
[0167] 2. Palletizing
[0168] Except that 5 temperature sensor groups are arranged at the drying medium inflow end and the outflow end of the material pile, all the other are the same as embodiment 1;
[0169] 3. Wood pretreatment
[0170] In addition to the heating stage of pretreatment except step B1) in the pretreatment process, that is, when the medium temperature is lower than 90°C (usually 70-90°C):
[0171] B1-1) When T 表 –T 中 When >5°C (usually 5-8°C), the heater is turned off, waiting for the temperature of the wood core to continue to rise;
[0172] B1-2) When T 表 –T 中 When ≤2°C (usually 2-4°C), turn on the heater and heat up at a heating rate of 10°C / h (usually 5-10°C / h);
[0173] Wherein, in the heating stage, steps B1-1) and B1-2) are carried out alternately until the temperature of the drying medium in the drying chamber reaches and re...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com