Oil immersion rust prevention method for cast iron pan
A technology of cast iron pot and anti-rust formula, which is applied to the surface coating liquid device, pretreatment surface, coating, etc., can solve the problems of easy rust, troublesome handling, etc., achieve uniform heat transfer, convenient maintenance, increase The effect of health function
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0013] Embodiment 1: the oil immersion antirust formula of the oil immersion antirust method of a kind of cast iron pan is: 10 parts of lard, 60-70 parts of peanut oil, 20-30 parts of palm oil; Its processing method is:
[0014] ① First remove the burrs from the cast iron pot, polish and clean it, and there should be no trachoma or scratches. You must wear gloves when operating, and then drill;
[0015] ② Mix the above-mentioned raw material oil again, pour it into the electric heating container, heat the oil temperature to 200°C, put it into the pot body, the hot oil should submerge the whole pot body, after the oil is heated to 235°C-255°C, heat it for 50°C -70 minutes, until the oil temperature is heated to 280-300°C, soak in hot oil for 72 hours;
[0016] ③Then take out the oil-soaked and anti-rust treated pot, and wipe the oil evenly with oil paper;
[0017] ④Put the cleaned pan into the oven to bake at 265°C-285°C for 40-60 minutes, take it out until completely cooled; ...
Embodiment 2
[0019] Embodiment 2: the oil immersion antirust formula of a kind of antirust treatment method of cast iron pan is: 10 parts of lard, 65 parts of peanut oils, 25 parts of palm oils; Its treatment method is:
[0020] ① First remove the burrs from the cast iron pot, polish and clean it, and there should be no trachoma or scratches. You must wear gloves when operating, and then drill;
[0021] ② Mix the above-mentioned raw material oil again, pour it into an electric heating container, heat the oil temperature to 200°C, put it into the pot body, the hot oil should submerge the whole pot body, after the oil is heated to 245°C, heat it for 60 minutes until Heat the oil to 280°C and soak in hot oil for 72 hours;
[0022] ③Then take out the oil-immersed anti-rust treated pot, and wipe the oil evenly with oil paper;
[0023] ④Put the cleaned pan into the oven to bake at 275°C for 50 minutes, take it out until completely cooled;
[0024] ⑤Finally, after fixing the pot handle with sta...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com