A technology for pumping concrete and construction methods, which is applied in the processing of building materials, construction, building construction, etc. It can solve the problems of fewer pipelines and blockages, and achieve the effects of reducing consumption, reducing resistance, and not being easy to block
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0034] The required concrete strength is C24.
[0035] Step 1, configure pumped concrete;
[0036] The pumped concrete is composed of the following raw materials in terms of mass percentage: 14% cement, 26% sand, 50% gravel, 10% water, and the sum of the mass percentages of the above components is 100%;
[0037] Step 2, configuring dry hard concrete;
[0038] Dry hard concrete is composed of the following raw materials in terms of mass percentage: 14% cement, 29% sand, 50% gravel, 7% water, and the sum of the mass percentages of the above components is 100%;
[0039] Step 1 and Step 2 use 32.5 grade ordinary Portland cement.
[0040] Step 3, pouring;
[0041] Pour the pumped concrete configured in step 1 and the dry hard concrete configured in step 2 respectively according to the ratio of 3.5:1;
[0042] Step 4, vibration;
[0043] Use the concrete vibrator to vibrate the pumped concrete and dry hard concrete poured in step 3, that is, the construction of the pumped concr...
Embodiment 2
[0045] The required concrete strength is C26.
[0046] Step 1, configure pumped concrete;
[0047] The pumped concrete is composed of the following raw materials in terms of mass percentage: 15% cement, 28% sand, 48% gravel, 9% water, and the sum of the mass percentages of the above components is 100%;
[0048] Step 2, configuring dry hard concrete;
[0049] Dry hard concrete is composed of the following raw materials in terms of mass percentage: 15% cement, 27% sand, 51% gravel, 7% water, and the sum of the mass percentages of the above components is 100%;
[0050] Step 1 and Step 2 use 42.5 grade ordinary Portland cement.
[0051] Step 3, pouring;
[0052] Pour the pumped concrete configured in step 1 and the dry hard concrete configured in step 2 respectively according to the ratio of 3.5:1;
[0053] Step 4, vibration;
[0054] Use the concrete vibrator to vibrate the pumped concrete and dry hard concrete poured in step 3, that is, the construction of the pumped concre...
Embodiment 3
[0056] The required concrete strength is C30.
[0057] Step 1, configure pumped concrete;
[0058] The pumped concrete is composed of the following raw materials in terms of mass percentage: 16% cement, 27% sand, 48% gravel, 9% water, and the sum of the mass percentages of the above components is 100%;
[0059] Step 2, configuring dry hard concrete;
[0060] Dry hard concrete is composed of the following raw materials in terms of mass percentage: 16% cement, 27% sand, 50% gravel, 7% water, and the sum of the mass percentages of the above components is 100%;
[0061] Step 1 and Step 2 use 42.5 grade ordinary Portland cement.
[0062] Step 3, pouring;
[0063] According to the ratio of 4:1, respectively pour the pumped concrete configured in step 1 and the dry hard concrete configured in step 2;
[0064] Step 4, vibration;
[0065] Use the concrete vibrator to vibrate the pumped concrete and dry hard concrete poured in step 3, that is, the construction of the pumped concret...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com