A technology of micro-arc oxidation and plasma, which is applied in the direction of anodic oxidation, etc., can solve the problems that the inner and outer surfaces of the pores cannot be treated at the same time, it is difficult to improve the efficiency, and increase the processing performance, so as to avoid electrolyte splashing, high oxidation treatment efficiency, and reduce dispersion current. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0010] Handling Workpieces: Gauge Aluminum Alloy Parts
[0011] Material model: duralumin LY12
[0012] Electrolyte formula: sodium silicate 10g / L
[0013] Sodium hydroxide 2.5g / L
[0014] Sodium Hexametaphosphate 1.5g / L
[0015] pH 12
[0016] Oxidation conditions: frequency 400Hz
[0017] Voltage: positive pulse peak voltage 400V
[0018] Negative pulse peak voltage 30V
[0019] Duty cycle 50%
[0020] Current density 8A / dm 2
[0021] Time 10min
[0022] Result: The film is dark gray, uniform and smooth, and the film thickness is 8μm to meet the requirements of use
Embodiment 2
[0024] Material model: duralumin LY12
[0025] Electrolyte formula: sodium silicate 10g / L
[0026] Sodium hydroxide 2.5g / L
[0027] Sodium borate 5g / L
[0028] Sodium tungstate 2g / L
[0029] pH 12
[0030] Oxidation conditions: frequency 400Hz
[0031] Voltage: positive pulse peak power 500V
[0032] Negative pulse peak voltage 40V
[0033] Duty cycle 50%
[0034] Current density 15A / dm 2
[0035] Time 360min
[0036] Result: Film thickness 200μm
[0037] Film hardness HV 2200
Embodiment 3
[0039] Select the inner hole parts (Φ18mmx50mm) as the processing workpiece.
[0040] Material model: deformed aluminum 8011
[0041] Electrolyte formula: sodium silicate 15g / L
[0042] Sodium hydroxide 5g / L
[0043] Sodium Hexametaphosphate 2g / L
[0044] Potassium sodium tartrate 1g / L
[0045] pH 13
[0046] Oxidation conditions: frequency 400Hz
[0047] Voltage: positive pulse peak voltage 300V
[0048] Negative pulse peak voltage 65V
[0049] Duty factor 30%
[0050] Current density 8A / dm 2
[0051] Auxiliary cathode 3mm diameter stainless steel wire
[0052]Time 10min
[0053] Result: The inner and outer surfaces were light gray, uniform in color, and the thickness of the surface smooth was 6 μm.
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
hardness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com