An offset printing ink and mineral oil technology, applied in the field of offset printing, can solve the problems of low ink roller sticking viscosity, offset printing ink sticking, etc., achieve the effect of high molecular weight, good water resistance and light fastness, and reduce cleaning and maintenance costs
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0049] The magenta ink described in this embodiment has the following components:
[0050] 73.775 kg of connecting material;
[0051] 1.5 kg of wax paste;
[0052] Pigments include 13 kg for Baohong 6BN and 5.5 kg for Baohong 8B, totaling 18.5 kg;
[0053] Anti-skinning agent 0.15 kg;
[0054] Auxiliary A includes 4.5 kg of viscosity modifier, 0.5 kg of anti-emulsification auxiliary, 0.3 kg of flow aid, 0.5 kg of antiwear agent, 0.025 kg of cobalt dry liquid, and 0.25 kg of manganese dry liquid, totaling 6.075 kg.
[0055] The connecting material, its components and parts by weight of each component are:
[0056] 44 parts of rosin modified octylphenol phenolic resin;
[0057] 24 parts of linseed oil;
[0058] 30 parts of mineral oil;
[0059] 1.1 parts of resin oil;
[0060] 0.2 parts of myristyl alcohol;
[0061] Additive B includes 0.6 part of liquid gelling agent and 0.1 part of BHT, 0.7 parts in total.
[0062] The wax paste, its components and parts by weight of each component are:
[0063]...
Embodiment 2
[0072] The medium yellow ink described in this embodiment has the following components:
[0073] 75.845 kg of connecting material;
[0074] 1.5 kg of wax paste;
[0075] The pigment is 178-1 yellow, 18.5 kg;
[0076] Anti-skinning agent 0.15 kg;
[0077] Auxiliary A includes 2.5 kg of viscosity modifier, 0.5 kg of anti-emulsification auxiliary, 0.3 kg of flow aid, 0.5 kg of antiwear agent, 0.03 kg of cobalt dry liquid, and 0.175 kg of manganese dry liquid, totaling 4.005 kg.
[0078] The connecting material, its components and parts by weight of each component are:
[0079] 40 parts of rosin modified octylphenol phenolic resin;
[0080] 30 parts of linseed oil;
[0081] 28 parts of mineral oil;
[0082] 1.8 parts of resin oil;
[0083] 0.1 part of myristyl alcohol;
[0084] Auxiliary B is 0.1 part of liquid gel, 0.1 part in total.
[0085] The wax paste, its components and parts by weight of each component are:
[0086] 3 parts linseed oil;
[0087] 75 parts of mineral oil;
[0088] 22 parts of be...
Embodiment 3
[0095] The sky blue ink described in this embodiment has the following components:
[0096] 78.775 kg of connecting material;
[0097] 2 kg of wax paste;
[0098] The pigment is 94817 blue 17.5 kg;
[0099] Anti-skinning agent 0.15 kg;
[0100] Auxiliary A includes 0.5 kg of anti-emulsification auxiliary, 0.3 kg of flow aid, 0.6 kg of antiwear agent, 0.025 kg of cobalt dry liquid, and 0.15 kg of manganese dry liquid, totaling 1.575 kg.
[0101] The connecting material, its components and parts by weight of each component are:
[0102] Rosin modified octylphenol phenolic resin 50 parts;
[0103] 20 parts of linseed oil;
[0104] 27 parts of mineral oil;
[0105] 1.7 parts of resin oil;
[0106] 0.3 parts of myristyl alcohol;
[0107] Auxiliary B includes 0.7 part of liquid gelling agent and 0.3 part of BHT, 1 part in total.
[0108] The wax paste, its components and parts by weight of each component are:
[0109] 8 parts linseed oil;
[0110] 72 parts of mineral oil;
[0111] 20 parts of beeswax.
...
PUM
Property | Measurement | Unit |
---|---|---|
Fineness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com