ABS color masterbatch and preparation method thereof
A color masterbatch and toner technology, applied in the field of plastic coloring, can solve the problems of increasing production cost, difficult to control color difference, large environmental pollution, etc., and achieve the effects of increasing safety, small color difference, and high color stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0025] This embodiment provides an ABS color masterbatch and a preparation method thereof, wherein the ABS color masterbatch is composed of the following raw materials in parts by mass:
[0026] 30 parts of carrier, 10 parts of inorganic pigment, 5 parts of maleic anhydride grafted polyethylene wax, 0.1 part of heat stabilizer, 1 part of polyethylene glycol and stearate, 15 parts of calcium oxide coated on the surface, flame retardant modified 10 parts of active agent, 5 parts of ultraviolet absorber, 3 parts of monoglyceride stearate;
[0027] Wherein, the carrier is prepared by mixing acrylonitrile, 1,3-butadiene, and styrene resin in a ratio of 2:1.2:5; quality chlorinated polyethylene; the ultraviolet absorber is composed of o-tert-butyl p-cresol, p-chloro-o-nitroaniline, organic silicon modified acrylic resin, bisphenol A diglycidyl ether and acrylic acid polyol according to 0.2:0.5: 2:0.7:1 ratio composition.
[0028] The preparation method of this ABS masterbatch comp...
Embodiment 2
[0031] 50 parts of carrier, 20 parts of organic pigment, 20 parts of maleic anhydride grafted polypropylene wax, 1 part of heat stabilizer, 5 parts of polyethylene glycol, 50 parts of activated hydrotalcite, 20 parts of flame retardant modifier, ultraviolet absorber 7 parts, 5 parts of polyethylene glycol oleate;
[0032] Wherein, the carrier is prepared by mixing acrylonitrile, 1,3-butadiene, and styrene resin in a ratio of 2:1.2:5; quality chlorinated polyethylene; the ultraviolet absorber is composed of o-tert-butyl p-cresol, p-chloro-o-nitroaniline, organic silicon modified acrylic resin, bisphenol A diglycidyl ether and acrylic acid polyol according to 0.2:0.5: 2:0.7:1 ratio composition.
[0033] The preparation method of this ABS masterbatch comprises the following steps:
[0034] The components are proportioned in proportion, and then mixed in a high-speed mixer for 15 minutes. The twin-screw extruder is used for melt blending. The temperature is controlled at 280 ° C...
Embodiment 3
[0036] 70 parts of carrier, 30 parts of white mineral oil, 20 parts of maleic anhydride grafted polyethylene wax, 20 parts of maleic anhydride grafted polypropylene wax, 2 parts of heat stabilizer, 10 parts of barium sulfate, 70 parts of dye, flame retardant modification 30 parts of neutralizing agent, 8 parts of ultraviolet absorber, 7 parts of polyethylene oxide;
[0037] Wherein, the carrier is prepared by mixing acrylonitrile, 1,3-butadiene, and styrene resin in a ratio of 2:1.2:5; quality chlorinated polyethylene; the ultraviolet absorber is composed of o-tert-butyl p-cresol, p-chloro-o-nitroaniline, organic silicon modified acrylic resin, bisphenol A diglycidyl ether and acrylic acid polyol according to 0.2:0.5: 2:0.7:1 ratio composition.
[0038] The preparation method of this ABS masterbatch comprises the following steps:
[0039] The components are proportioned, then mixed in a high-speed mixer for 20 minutes, melt blended with a twin-screw extruder, the temperature...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com