A formaldehyde scavenger and formaldehyde scavenger technology, applied in physical/chemical process catalysts, organic compound/hydride/coordination complex catalysts, dispersed particle separation, etc., can solve secondary pollution, limited formaldehyde removal effect, environmental problems Pollution and other problems, to achieve the effect of mild application conditions
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0037] A formaldehyde scavenger is composed of the following components in weight percentage: 8g of manganese oxide supported on activated carbon, 8g of 2-imidazolidinone, 8g of diatomaceous earth supported titanium dioxide, 0.1g of nano-silver colloid, and 75.9g of pure water.
[0038] The preparation process is as follows:
[0039] (1) Take diatomite-loaded titanium dioxide and nano-silver colloid in the formula amount and add them to 35.9g of pure water, mix and stir for 30 minutes to obtain a mixed solution;
[0040] (2) Add activated carbon-supported manganese oxide and 2-imidazolidinone in the formula amount to 40 g of pure water, stir evenly to obtain a mixed solution;
[0041] (3) Add the mixed solution obtained in step (2) to the mixed solution obtained in step (1), and stir for 30 minutes to obtain the finished product.
Embodiment 2
[0043]A formaldehyde scavenger, consisting of the following components by weight percentage: activated carbon supported manganese oxide 8g, 1-(2-hydroxyethyl)-2-imidazolidinone 8g, diatomaceous earth supported titanium dioxide 8g, nano silver colloid 0.1g , Pure water 75.9g.
[0044] The preparation process is as follows:
[0045] (1) Take diatomite-loaded titanium dioxide and nano-silver colloid in the formula amount and add them to 35.9g of pure water, mix and stir for 30 minutes to obtain a mixed solution;
[0046] (2) Take the activated carbon-loaded manganese oxide and 1-(2-hydroxyethyl)-2-imidazolidinone in the formula amount and add them to 40g of pure water, stir evenly to obtain a mixed solution;
[0047] (3) Add the mixed solution obtained in step (2) to the mixed solution obtained in step (1), and stir for 30 minutes to obtain the finished product.
Embodiment 3
[0049] A formaldehyde scavenger, consisting of the following components by weight percentage: activated carbon supported manganese oxide 8g, 2-imidazolidinone 4g, 1-(2-hydroxyethyl)-2-imidazolidinone 4g, diatomaceous earth supported titanium dioxide 8g, nano silver glue 0.1g, pure water 75.9g.
[0050] The preparation process is as follows:
[0051] (1) Take diatomite-loaded titanium dioxide and nano-silver colloid in the formula amount and add them to 35.9g of pure water, mix and stir for 30 minutes to obtain a mixed solution;
[0052] (2) Take the activated carbon-supported manganese oxide, 2-imidazolidinone, and 1-(2-hydroxyethyl)-2-imidazolidinone in the formula amount and add them to 40 g of pure water, stir evenly to obtain a mixed solution;
[0053] (3) Add the mixed solution obtained in step (2) to the mixed solution obtained in step (1), and stir for 30 minutes to obtain the finished product.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com