ZSM-5 molecular sieve and preparation method thereof
A technology of ZSM-5 and molecular sieve, which is applied in the direction of crystalline aluminosilicate zeolite, borocarbane silicone crystalline aluminosilicate zeolite, etc., can solve the problem of high preparation cost, difficulty in meeting the needs of acidic properties, and high price of organic templates and other issues to achieve the effect of low synthesis cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0020] In the first step, add sodium hydroxide and aluminum sulfate into deionized water respectively, stir for half an hour, add silica sol, stir evenly, put it into a stainless steel crystallization kettle, crystallize at a constant temperature of 170°C for 60 hours, and then cool to room temperature .
[0021] The second step is to stir the cooled mixture after crystallization. After stirring evenly, add aluminum sulfate directly, then stir for 2 hours, put it into a stainless steel crystallization kettle, and crystallize at a constant temperature of 178°C for 48 hours, then cool to room temperature, and wash , drying and roasting to obtain ZSM-5 molecular sieve.
[0022] The molar ratio of synthetic raw materials is (excluding the aluminum source added in the second step): Al 2 o 3 :60SiO2 2 :9.4Na 2 O:3778H 2 O. The aluminum source that the second step adds is the 62% of the first step (mass percentage, with Al 2 o 3 count).
Embodiment 2
[0027] The first step is to add sodium hydroxide and aluminum sulfate into deionized water respectively, stir for half an hour, add silica sol, stir well, put it into a stainless steel crystallization kettle, crystallize at a constant temperature of 170°C for 72 hours, and then cool to room temperature .
[0028] The second step is to stir the cooled mixture after crystallization. After stirring evenly, add aluminum nitrate directly, then stir for 2 hours, put it into a stainless steel crystallization kettle, crystallize at a constant temperature of 175°C for 36 hours, then cool to room temperature, and wash , drying and roasting to obtain ZSM-5 molecular sieve.
[0029] The molar ratio of synthetic raw materials is (excluding the aluminum source added in the second step): Al 2 o 3 :60SiO2 2 :9.4Na 2 O:3778H 2 O. The aluminum source that the second step adds is 60% of the first step (mass percentage, with Al 2 o 3 count).
Embodiment 3
[0031] In the first step, sodium hydroxide and aluminum sulfate are added to deionized water respectively, and after stirring for half an hour, silica sol is added. After stirring evenly, put it into a stainless steel crystallization kettle, crystallize at a constant temperature of 170°C for 60 hours, and then cool to room temperature .
[0032] The second step is to stir the cooled mixture after crystallization. After stirring evenly, add aluminum sulfate directly, then stir for 2 hours, put it into a stainless steel crystallization kettle, and crystallize at a constant temperature of 170°C for 60 hours, then cool to room temperature, and wash , drying and roasting to obtain ZSM-5 molecular sieve.
[0033] The molar ratio of synthetic raw materials is (excluding the aluminum source added in the second step): Al 2 o 3 :90SiO2 2 :9.4Na 2 O:3780H 2 O. The aluminum source that the second step adds is the 77% of the first step (mass percentage, with Al 2 o 3 count).
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com