[0025] An environmentally friendly leather finishing agent, prepared from the following raw materials in weight percentage: 25% ethyl acrylate, 3% acrylic acid, 5% sodium lauryl sulfate, 0.2% potassium persulfate, 0.3% sodium dithionite, Zinc oxide 5%, the balance is water.
[0026] The preparation method of this leather finishing agent, comprises the following steps:
[0027] S1. Mix ethyl acrylate, acrylic acid and emulsifier evenly, and pre-emulsify for 1 hour to obtain a pre-emulsion;
[0028] S2, adding the initiator into water and mixing uniformly to obtain an aqueous solution of the initiator;
[0029] S3. Add the aqueous initiator solution to the pre-emulsion to initiate polymerization. When the temperature drops to 50°C, add zinc oxide to the reaction solution and mix evenly. When the temperature drops to 25°C, add an appropriate amount of Adjust the pH value to 7.2 with ammonia water and cool down to room temperature to obtain a leather finishing agent.
[0030] A...
Embodiment 2
[0032] An environmentally friendly leather finishing agent, prepared from the following raw materials in weight percentage: 15% ethyl acrylate, 1% acrylic acid, 3% sodium lauryl sulfate, 0.1% potassium persulfate, 0.1% sodium dithionite, Zinc oxide 2%, the balance is water.
[0033] The preparation method of this leather finishing agent, comprises the following steps:
[0034] S1. Mix ethyl acrylate, acrylic acid and emulsifier evenly, and pre-emulsify for 0.5h to obtain a pre-emulsion;
[0035] S2, adding the initiator into water and mixing uniformly to obtain an aqueous solution of the initiator;
[0036] S3. Add the aqueous initiator solution to the pre-emulsion to initiate polymerization. When the temperature drops to 45°C, add zinc oxide to the reaction solution and mix evenly. When the temperature drops to 20°C, add an appropriate amount of Adjust the pH value to 7.1 with ammonia water and cool down to room temperature to obtain a leather finishing agent.
[0037] Acc...
Embodiment 3
[0039] An environmentally friendly leather finishing agent prepared from the following raw materials in weight percentage: 40% ethyl acrylate, 8% acrylic acid, 10% sodium lauryl sulfate, 0.4% ammonium persulfate, and 0.4% sodium bisulfite , zinc oxide 8%, the balance is water.
[0040]The preparation method of this leather finishing agent, comprises the following steps:
[0041] S1. Mix ethyl acrylate, acrylic acid and emulsifier evenly, and pre-emulsify for 1.5 hours to obtain a pre-emulsion;
[0042] S2, adding the initiator into water and mixing uniformly to obtain an aqueous solution of the initiator;
[0043] S3. Add the aqueous initiator solution to the pre-emulsion to initiate polymerization. When the temperature drops to 55°C, add zinc oxide to the reaction solution and mix evenly. When the temperature drops to 30°C, add an appropriate amount of Adjust the pH value to 7.3 with ammonia water and cool down to room temperature to obtain a leather finishing agent.
[00...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com